Skip to main content
. 2008 May 1;43(10):3689–3696. doi: 10.1007/s10853-008-2592-3

Table 2.

Tensile results for PTMO2000-T6A6T at various temperatures, ηinh = 2.2 dL/g

Temperature G′ (MPa) E-Modulus (MPa) E/G′ (−) σ10% (MPa) σy (MPa) ɛy (%) σb (MPa) ɛb (%) σ atrue (MPa)
20 °C 20 53 2.7 4.5 8.7 49 29 480 165
50 °C 20 59 3.0 3.8 7.2 42 22 550 143
80 °C 18 56 3.1 3.4 5.8 37 17 490 98
110 °C 16 53 3.3 2.9 4.7 33 12 400 61

a σtrue was obtained by multiplying σbreak with the straining factor (=1 +  (ɛbreak/100))