Table 5.

Hardened mortar prisms with kneading water replaced by different percentages of lime solution.

Mortar Specimens Tensile Strength (MPa) Compressive Strength (MPa)
M_0% 0.79 0.86 ± 0.09 1.49 1.98 ± 0.32
0.99 1.73
0.79 2.22
0.80 2.43
0.95 2.26
-- 1.75
M_5% 1.07 1.11 ± 0.04 2.28 2.40 ± 0.11
1.08 2.36
1.19 2.55
1.12 2.55
1.08 2.43
-- 2.21
M_10% 1.37 1.34 ± 0.06 3.77 3.23 ± 0.19
1.25 3.13
1.39 3.19
1.28 2.95
1.39 3.27
-- 3.06
M_15% 1.28 1.40 ± 0.11 4.34 3.88 ± 0.28
1.59 3.73
1.33 3.97
1.49 3.84
1.31 3.22
-- 4.18