Table 4.

Values for 30 × 30 × 30 mm PP and GFPP cubes autoclaved at 134 °C. PP cubes withstood one and two rounds of autoclaving at this temperature. GFPP cubes displayed a larger variance because some cubes melted after two rounds of autoclaving, but others survived one and three rounds. Numbers in parentheses denote a negative calculated value

Polymer Number of Autoclaves Completed Average Initial Mass (g) Average Percent Mass Loss Average Percent Volume Loss Category
PP (n = 5) 1 14.46 ± 0.19 0.04 % ± 0.008 % 0.33 % ± 0.34 % 1
PP (n = 10) 2 14.63 ± 0.20 0.01 % ± 0.007 % 0.87 % ± 0.58 % 1
PP (n = 5) 3 14.53 ± 0.06 0.06 % ± 0.016 % 1.70 % ± 1.81 % 2

GFPP

(n = 5)

1 16.16 ± 0.23 (0.01)% ± 0.008 % 0.43 % ± 0.37 % 1

GFPP

(n = 10)

2 16.06 ± 0.16 0.06 % ± 0.38 % 4.04 % ± 4.27 % 3

GFPP

(n = 5)

3 15.91 ± 0.11 (0.03)% ± 0.03 % 0.60 % ± 0.46 % 1