. 2021 Aug 11;11(8):2041. doi: 10.3390/nano11082041

Table 1.

The specific surface area, pore size, and elemental composition of GCN-B and GCNs that recalcined at different temperatures.

Sample d-Spacing (Å) SBET (m2/g) Pore Size (nm) Pore Volume(cm3/g) Elemental Composition C/N Ratio Yield Remained after Recalcination (%)
(002) (100) C (wt%) N (wt%)
GCN-B 3.244 6.783 30.20 3.68 0.083 35.10 51.53 0.681 100
GCN-450 3.220 6.781 79.96 3.49 0.144 35.68 50.33 0.708 73
GCN-500 3.194 6.782 117.05 3.59 0.210 37.71 52.38 0.720 45
GCN-550 3.188 6.781 158.57 3.63 0.228 38.76 47.87 0.809 18