Table 6.
(a) Descriptive statistics of indentation hardness, stiffness and indentation modulus of the surface of the tested materials—materials without aging; (b) Descriptive statistics of indentation hardness, stiffness and indentation modulus of the surface of the tested materials—materials after aging.
(a) Descriptive Statistics of Indentation Hardness, Stiffness and Indentation Modulus of the Surface of the Tested Materials—Materials without Aging | ||||||
Mechanical Size | Statistical Parameter | Materials without Aging | ||||
M I | M II | M III | M V | M VI | ||
N (no. of. specim.) = 5 | n (no. of. obs.) | 25 | 25 | 25 | 25 | 25 |
HIT (O & P) [MPa] |
Mean | 78.414 | 84.475 | 81.767 | 254.001 | 116.568 |
Std Dev | 1.437 | 1.445 | 1.795 | 21.086 | 5.63 | |
Min. | 76.06 | 80.087 | 77.102 | 211.728 | 107.606 | |
Max. | 81.377 | 86.927 | 85.799 | 289.394 | 129.209 | |
Median | 78.207 | 84.652 | 82.169 | 249.701 | 116.89 | |
Shape (Weibull) | 61.572 | 67.557 | 52.147 | 13.893 | 23.579 | |
Scale (Weibull) | 79.104 | 85.153 | 82.614 | 263.37 | 119.18 | |
S (O & P) [mN/μm] |
Mean | 383.728 | 315.936 | 372.101 | 420.71 | 1170.405 |
Std Dev | 4.023 | 2.557 | 1.971 | 3.103 | 126.55 | |
Min. | 374.736 | 311.198 | 368.443 | 414.862 | 682.258 | |
Max. | 390.423 | 320.156 | 377.42 | 426.686 | 1394.335 | |
Median | 384.018 | 315.211 | 371.749 | 420.5 | 1183.031 | |
EIT (O & P) [GPa] |
Mean | 1.918 | 1.639 | 1.899 | 3.788 | 7.16 |
Std Dev | 0.033 | 0.023 | 0.027 | 0.172 | 0.757 | |
Min. | 1.87 | 1.585 | 1.825 | 3.433 | 4.21 | |
Max. | 1.989 | 1.672 | 1.953 | 4.088 | 8.57 | |
Median | 1.911 | 1.638 | 1.9 | 3.742 | 7.229 | |
E* (O & P) [GPa] |
Mean | 2.108 | 1.801 | 2.086 | 4.163 | 7.868 |
Std Dev | 0.036 | 0.025 | 0.03 | 0.189 | 0.832 | |
Min. | 2.055 | 1.742 | 2.006 | 3.772 | 4.627 | |
Max. | 2.185 | 1.838 | 2.146 | 4.492 | 9.417 | |
Median | 2.1 | 1.8 | 2.088 | 4.113 | 7.944 | |
(b) Descriptive statistics of indentation hardness, stiffness and indentation modulus of the surface of the tested materials—materials after aging | ||||||
Mechanical size | Statistical parameter | Materials after aging | ||||
M I AS | M II AS | M III AS | M V AS | M VI AS | ||
N (no. of. specim.) = 5 | n (no. of. obs.) | 25 | 25 | 25 | 25 | 25 |
HIT (O & P) [MPa] |
Mean | 51.565 | 67.722 | 50.664 | 219.804 | 189.726 |
Std Dev | 2.864 | 3.767 | 2.024 | 5.56 | 6.904 | |
Min. | 46.261 | 60.433 | 46.551 | 207.193 | 178.742 | |
Max. | 55.124 | 72.87 | 54.427 | 228.273 | 203.9 | |
Median | 52.154 | 68.128 | 50.89 | 219.878 | 188.594 | |
Shape (Weibull) | 20.454 | 20.66 | 29.162 | 46.17 | 31.090 | |
Scale (Weibull) | 52.889 | 69.442 | 51.588 | 222.37 | 192.99 | |
S (O & P) [mN/μm] |
Mean | 249.884 | 256.947 | 254.125 | 401.786 | 481.595 |
Std Dev | 2.7 | 5.212 | 2.931 | 5.267 | 5.916 | |
Min. | 245.445 | 244.751 | 248.441 | 393.725 | 472.935 | |
Max. | 254.98 | 263.548 | 260.178 | 410.869 | 489.864 | |
Median | 249.783 | 257.835 | 253.171 | 401.018 | 483.139 | |
EIT (O & P) [GPa] |
Mean | 1.011 | 1.193 | 1.02 | 3.366 | 3.75 |
Std Dev | 0.038 | 0.056 | 0.031 | 0.07 | 0.11 | |
Min. | 0.941 | 1.073 | 0.956 | 3.208 | 3.602 | |
Max. | 1.067 | 1.268 | 1.07 | 3.48 | 3.956 | |
Median | 1.025 | 1.199 | 1.014 | 3.365 | 3.753 | |
E* (O & P) [GPa] |
Mean | 1.112 | 1.311 | 1.121 | 3.698 | 4.121 |
Std Dev | 0.042 | 0.062 | 0.034 | 0.077 | 0.121 | |
Min. | 1.034 | 1.179 | 1.05 | 3.526 | 3.958 | |
Max. | 1.173 | 1.394 | 1.175 | 3.824 | 4.348 | |
Median | 1.126 | 1.318 | 1.114 | 3.698 | 4.124 |