Skip to main content
. 2021 Aug 10;13(16):2650. doi: 10.3390/polym13162650

Table 3.

Results of tensile tests on PHBHV/MIS composites considering different fiber content (0, 5, 10, 20, 30 wt %). The standard deviation values are also presented.

Samples Tensile Modulus [MPa] Tensile Strength [MPa] Ultimate Strain [%]
PHBHV 889 ± 41 22.0 ± 0.48 9.9 ± 1.1
PHBHV95MIS5 1074 ± 44 17.0 ± 1.54 4.2 ± 0.7
PHBHV90MIS10 1238 ± 74 16.8 ± 1.67 4.4 ± 0.9
PHBHV80MIS20 1267 ± 90 15.8 ± 0.77 3.9 ± 0.2
PHBHV70MIS30 1891 ± 172 16.9 ± 1.03 3.3 ± 0.7