Table 6.
Flexural strength and compressive strength of nano-Al2O3 particle blended cement mortars.
Sample Designation | Flexural Strength, MPa | Compressive Strength, MPa | ||||
---|---|---|---|---|---|---|
7 Days | 28 Days | 90 Days | 7 Days | 28 Days | 90 Days | |
MNA-0 | 6.1 ± 0.14 | 7.4 ± 0.33 | 7.8 ± 0.33 | 28.2 ± 0.30 | 36.9 ± 0.61 | 42.0 ± 0.65 |
MNA-1 | 6.1 ± 0.17 | 7.5 ± 0.33 | 8.2 ± 0.12 | 34.1 ± 1.14 | 39.5 ± 0.42 | 47.3 ± 1.17 |
MNA-2 | 6.0 ± 0.18 | 7.1 ± 0.33 | 8.0 ± 0.37 | 32.4 ± 0.51 | 40.0 ± 0.55 | 46.3 ± 0.73 |
MNA-3 | 5.7 ± 0.09 | 6.8 ± 0.33 | 7.7 ± 0.10 | 31.6 ± 0.5 | 39.6 ± 0.78 | 44.6 ± 0.59 |
MNA-4 | 5.6 ± 0.32 | 6.9 ± 0.33 | 7.2 ± 0.45 | 29.9 ± 1.28 | 36.8 ± 1.08 | 44.1 ± 1.07 |