Table 4.
Specimen | Benchmark | Kevlar/Carbon HFRC Specimen (L12 mm/L24 mm) | ||||||
---|---|---|---|---|---|---|---|---|
C-B | C-K10/C0 | C-K8/C2 | C-K6/C4 | C-K5/C5 | C-K4/C6 | C-K2/C8 | C-K0/C10 | |
Compressive Strength (MPa) | 22.13 | 29.60 | 30.77 | 32.13 | 31.97 | 30.25 | 29.01 | 27.26 |
23.97 | 31.54 | 32.64 | 33.01 | 33.14 | 31.11 | 29.19 | 28.60 | |
23.98 | 31.61 | 33.11 | 33.60 | 33.24 | 32.72 | 29.98 | 28.83 | |
Average
Compressive Strength (MPa) |
23.36 | 30.92 | 32.18 | 32.91 | 32.78 | 31.36 | 29.39 | 28.23 |
Increase (%) | - | 32 | 28 | 41 | 40 | 34 | 26 | 21 |