Table 2.
Summary of the spherulite size and crystallinity measurements of LDPE injection-molded specimens.
Injection Molding Condition (Melt–Mold) |
Spherulite | Crystallinity | ||
---|---|---|---|---|
Average Size (μm) | Std. Dev. (μm) | Ratio (A/C) | X (%) | |
120–10 | 7.03 | 1.80 | 0.26 | 31.5 |
120–40 | 6.87 | 2.17 | 0.26 | 29.8 |
120–80 | 6.64 | 2.68 | 0.27 | 31.5 |
140–10 | 11.46 | 3.53 | 0.27 | 33.6 |
140–40 | 8.39 | 2.30 | 0.26 | 33.9 |
140–80 | 7.76 | 2.18 | 0.26 | 32.2 |
160–10 | 10.88 | 4.32 | 0.26 | 33.5 |
160–40 | 6.28 | 2.25 | 0.26 | 31.4 |
160–80 | 8.35 | 2.34 | 0.28 | 31.7 |