Skip to main content
. 2021 Nov 7;26(21):6734. doi: 10.3390/molecules26216734

Table 3.

Water vapor transmission rate (WVTR) and water vapor permeability (WVP) of starch-polyvinyl alcohol (SP) film reinforced with nanoclays (MMT), sonicated with ultrasound.

Film Sample WVTR
g·mm/(m2·day)
WVP
g/(m2·day)
SP 1073.2170 4658.290
SP0.5MMT-s 331.3667 3122.959
SP1.0MMT-s 736.2055 3675.283
SP1.5MMT-s 884.4438 4836.468