Table 2.
Cathode Configuration | Areal Sulfur Loading (mg cm−2) |
Electrolyte | C Rate | Specific Capacity (mAh g−1) |
Ref. |
---|---|---|---|---|---|
Oxidized TiN–ordered mesoporous carbon/S | ~1.4 | DOL/DME | 0.1 | 884 | [41] |
Carbon cloth@carbon-encapsulated CoP nanosheet arrays/S | 3.4 | DOL/DGM | 0.1 | 1100 | [42] |
CoS2–sulfurized polyacrylonitrile–CNT | 5.9 | EC/DMC/DEC | 0.2 | ~1600 | [43] |
S@CNTs/CoS nanostraws | 3.8 | DOL/DME | 0.1 | 1330 | [24] |
CNT@nitrogen-enriched carbon/S | 4 | TEGDME | – | 1300 | [44] |
N-doped Ketjenblack/S | 2.4 | DOL/DME | – | ~900 | [45] |
Graphene foam–rGO/S | 10 | DOL/DME | 0.04 | 1235 | [26] |
Polar hierarchical–porous carbon container@S | 4 | DOL/DME | 0.2 | 733 | [46] |
S/(graphene–graphitic carbon nanocages) | 3 | DOL/DME | 0.05 | ~1000 | [35] |
S/conductive carbon | 4.5 | DOL/DME | 0.05 | 1490 | [47] |
S/Ketjenblack–Ni–P layers | 2 | DOL/DME | 0.1 | 1420 | [48] |
Pure sulfur cathode | ~10.4 | DOL/DME | 0.05 | 1160 | [49] |
Sulfurized carbonized polyacrylonitrile | 3 | EC/DEC | 0.5 | ~1300 | [50] |
1 The anode of pouch cells in Table 2 is metallic lithium.