Skip to main content
. 2021 Nov 19;13(22):3996. doi: 10.3390/polym13223996

Table 2.

Decomposition temperatures of the PLA/PA bioblends, at a nominal heating rate of 10 K/min.

T5 (°C) T95 (°C) αm Tm (°C) (/dT)m
(K−1)
αr Tr (°C) (/dT)r
(K−1)
PLA/PA 90/10 315.8 455.0 0.54 349.8 2.39·10−2 0.45 346.1 2.38·10−2
PLA/PA 80/20 317.4 554.4 0.43 343.1 2.49·10−2 0.40 341.8 2.46·10−2
PLA/PA 70/30 318.8 540.2 0.35 339.2 2.83·10−2 0.35 339.3 1.76·10−2
PLA/PA 60/40 320.5 484.1 0.30 338.5 2.69·10−2 0.30 338.4 0.49·10−2
PLA/PA 50/50 321.2 479.2 0.27 337.6 2.01·10−2 0.25 336.6 0.18·10−2