Table 4.
Measured residual stress on the surface and inside of as-sprayed and heat treated cold sprayed samples using X-ray diffractometry
| Sample Depth | Residual Stress, MPa | |||||
|---|---|---|---|---|---|---|
| Before heat treatment | After heat treatment | |||||
| Longitudinal (0°) | 45° | Transverse (90°) | Longitudinal (0°) | 45° | Transverse (90°) | |
| Inconel 625 Surface | 598 | 752 | 974 | −56 | −45 | −36 |
| Inconel 625 1 mm | −195 | −159 | −229 | −54 | −32 | −46 |
| Inconel 718 Surface | −160 | −65 | 27 | −161 | −193 | −158 |
| Inconel 718 1 mm | −199 | −133 | −225 | 35 | −20 | 7 |