Skip to main content
. 2021 Dec 3;14(23):7426. doi: 10.3390/ma14237426

Table 1.

Properties of SBS modified asphalt.

Test Indexes Requirements Results Experiment Method
Penetration (25 °C)/0.1 mm 60~80 71 T0604
Softening point/°C ≮55 86 T0606
Ductility (5 cm/min, 15 °C)/cm ≮30 48 T0605
Penetration Index (PI) −0.4~1.0 0.5 T0604
Segregation (soften the spread)/°C ≯2.5 1.4 T0661
Recovery of elasticity (25 °C)/% ≮65 76 T0662
RTFOT residue Quality change/% ±1.0 −0.08 T0610
Penetration ratio/% ≮60 86 T0604
15 °C residual ductility/cm ≮20 37 T0605