Table 2.
Comparison of mean values of tensile properties and surface roughness for as-received group (Subgroup 1) and nonfluoride control group (Subgroup 2)
| Group | Parameter | Mean±SD | P* | |
|---|---|---|---|---|
|
| ||||
| Subgroup - 1 | Subgroup - 2 | |||
| I (NiTi) | Tensile strength | 1328.8±32.6 | 1301.8±40.4 | 0.12 (NS) |
| Elongation rate | 21.1±0.9 | 21.0±0.7 | 0.79 (NS) | |
| Ra | 422.5±23.1 | 431.7±24.6 | 0.40 (NS) | |
| Rq | 549.5±22.5 | 573.2±27.3 | 0.048 (significant) | |
| II (heat activated NiTi) | Tensile strength | 1152.2±35.5 | 1135.5±26.7 | 0.25 (NS) |
| Elongation rate | 22.3±1.3 | 21.9±1.5 | 0.51 (NS) | |
| Ra | 411.0±35.7 | 456.8±34.7 | 0.009 (significant) | |
| Rq | 549.1±39.0 | 594.3±40.2 | 0.02 (significant) | |
| III (TMA) | Tensile strength | 1108.7±26.6 | 1086.9±28.5 | 0.10 (NS) |
| Elongation rate | 5.1±1.2 | 5.0±1.0 | 0.72 (NS) | |
| Ra | 427.8±40.9 | 464.7±35.5 | 0.045 (significant) | |
| Rq | 559.2±61.3 | 609.3±42.8 | 0.048 (significant) | |
Ra: Roughness average, Rq: Root mean square roughness, SD: Standard deviation, NS: Not significant, NiTi: Nickel Titanium, TMA: Titanium Molybdenum alloy