Skip to main content
. 2021 Dec 17;13(24):4431. doi: 10.3390/polym13244431

Table 1.

Thickness, water solubility, and water-vapor permeability of thermoplastic modified cornstarch and chitosan composite film.

Starch:Chitosan Volume Solution Ratios Thickness (µm) Solubility (%) Contact Angle (°) WVP × 10−11
(g·m−1·s−1·Pa−1)
TPS100-CH0 110.36 ± 1.61 d 30.70 ± 2.35 a 90.58 ± 0.40 d 26.20 ± 6.43 e
TPS75-CH25 162.54 ± 7.84 e 47.24 ± 2.07 b 86.08 ± 0.06 c 4.95 ± 0.81 c
TPS50-CH50 70.06 ± 0.95 b 49.86 ± 5.30 b 72.39 ± 0.51 b 5.74 ± 0.77 d
TPS25-CH75 90.46 ± 6.48 c 70.92 ± 7.42 c 56.79 ± 1.05 a 0.55 ± 0.03 a
TPS0-CH100 49.07 ± 2.59 a 68.84 ± 6.68 c 67.51 ± 2.02 b 4.01 ± 0.52 b

Values with a different letter in the same column denote significant difference (Tukey test; p < 0.05). Values are given as mean ± standard deviation (n = 10 for thickness and n = 3 for solubility, contact angle, and WVP).