Optimized conditions for aluminium-based (matrix) and MC (reinforcement) [31, 58, 66, 89102].

ES MAM-P M-R LP (W) SS (mm/s) LT (μm) HS (μm) BT (°C)
Laser SLM AlSi10Mg-3% TiC 80-140 200 50 50 100
Laser SLM AlSi10Mg-5% TiC 100 100-400 50 50
Laser SLM AlSi15-5% TiC 360 650 20 100
Laser DED AlSi10Mg-5% TiC 3000 10 2000
Laser DED AlSi10Mg-30 Vol% TiC 1800 7-17 100-200
Laser SLM Al9.8Si0.6MgTi- TiC 400 90
Laser SLM AlSi10Mg-5% TiC 320 1100 30 130
Laser SLM AlSi10Mg-15% SiC 500 600-2100 40 60-180
Laser SLM AlSi10Mg-5 Vol% SiC 195 640-880 30 500
Laser SLM AlSi10Mg-10 Vol% SiC 195 640-880 30 500
Laser SLM Al-15% SiC 500 50 100
Laser Laser sintering Al–7Si–0.3Mg—5 to 12 Vol % SiC 8.6 100 30 80
Laser SLM AlSi10Mg-20% SiC 200 100 30 50
Laser SLM Al7Si-10 Vol% SiC 200 500-1750 50 100
Laser SLM AlSi10Mg-20% B4C 100-200 100 50 130 to 150

ES: energy source; MAM-P: metal-based additive manufacturing; M-R: matrix-reinforcement; LP: laser power; SS: scanning speed; LT: layer thickness; HS: hatch spacing; BT: bed temperature.