Table 1.
Impurity levels in the doped ingots determined by GDMS analysis. Data for CdTe:P, CdTe:As, and CdTe:Na are shown in order from left. The units are PPB.
Elements | Top | Bottom | Elements | Top | Bottom | Elements | Top | Bottom |
---|---|---|---|---|---|---|---|---|
C | 400 | 310 | C | 410 | 310 | C | 390 | 300 |
N | 20 | 20 | N | 20 | 20 | N | 20 | 20 |
O | 700 | 810 | O | 720 | 790 | O | 700 | 710 |
Na | 20 | 140 | Na | 30 | 130 | Na | 7100 | 8000 |
Mg | 40 | 30 | Mg | 40 | 30 | Mg | 40 | 30 |
Al | 10 | 10 | Al | 10 | 10 | Al | 10 | 10 |
Si | 10 | 20 | Si | 10 | 20 | Si | 10 | 20 |
P | 17,000 | 18,000 | P | 80 | 60 | P | 80 | 60 |
S | 30 | 30 | S | 30 | 30 | S | 30 | 30 |
Cu | 40 | 80 | Cu | 30 | 70 | Cu | 30 | 70 |
As | 40 | 50 | As | 22,000 | 23,000 | As | 40 | 50 |