. 2022 Feb 21;2022:8353137. doi: 10.1155/2022/8353137

Table 2.

The means and standard deviations of the Vickers hardness and flexural strength values found for the 3D-printed material.

Postprinting treatment conditions 3D printing thickness
20 50 100
FS (mean ± SD) VHN (mean ± SD) FS (mean ± SD) VHN (mean ± SD) FS (mean ± SD) VHN (mean ± SD)
Dry storage (control) 91.51 (10.05)a 13.23 (0.48)a 94.40 (9.61)a 16.23 (0.22)a 91.51 (10.05)a 9.31 (0.22)a
WS for 24 h 68.38 (9.02)b 10.68 (1.67)a 88.25 (8.83)b 16.63 (0.10)a 68.38 (9.02)b 12.71 (2.97)a
WS for 1 month 64.37 (7.43)b 14.86 (1.85)a 77.67 (9.13)bc 16.38 (0.35)a 64.37 (7.43)b 13.90 (0.45)b
LC 5 min 80.80 (8.72)ab 14.33 (0.08)b 83.76 (10.44)c 16.63 (0.51)b 80.80 (8.72)ab 12.45 (1.41)a
LC 15 min 82.80 (9.09)ab 15.21 (0.12)a 91.02 (4.80)ab 16.20 (1.10)b 82.80 (9.09)ab 12.93 (0.42)ab
HC 5 min 71.32 (4.46)bc 13.46 (0.34)c 83.47 (12.08)bd 17.06 (0.30)c 71.32 (4.46)bc 17.95 (1.09)c
HC 15 min 64.83 (9.07)bd 12.41 (0.35)a 88.86 (8.03)bd 17.66 (0.81)d 64.83 (9.07)bd 14.88 (0.31)ad

FS: flexural strength; VHN: Vickers hardness. Same superscripted lowercase letters indicate groups not statistically significantly different when compared by Tukey's multiple comparison post hoc analysis (p > 0.05).