Table 4.

Textural properties of sterile aerogel-based scaffolds obtained from aqueous 6 wt.% alginate inks with different HA contents (0, 8, 16, 24 wt.%) and crosslinked by ageing with CaCl2 1M1h and by GA. Notation: ABET: specific BET surface area, dp: BJH-mean pore diameter, Vp: BJH-specific pore volume.

Sterile Aerogel Scaffold ABET (m2/g) dp (nm) Vp (cm3/g)
Alg 6%, HA 8%, CaCl2 1M1h, st 105 ± 5 28 ± 1 0.89 ± 0.04
Alg 6%, HA 16%, CaCl2 1M1h, st 68 ± 3 27 ± 1 0.52 ± 0.03
Alg 6%, HA 24%, CaCl2 1M1h, st 56 ± 3 26 ± 1 0.41 ± 0.02
Alg 6%, HA 8%, CaCl2 1M1h, GA, st 59 ± 3 25 ± 1 0.43 ± 0.02
Alg 6%, HA 16%, CaCl2 1M1h, GA, st 30 ± 2 29 ± 1 0.27 ± 0.01
Alg 6%, HA 24%, CaCl2 1M1h, GA, st 32 ± 2 23 ± 1 0.17 ± 0.01