Corrosion parameters obtained from potentiodynamic polarization measurements for C-steel in SCPS contaminated with 0.6 M NaCl in the absence and presence of various concentrations of EDTA at 25 °C.
| Sample | E corr vs. Ag/AgCl (mV) | I corr (μA cm−2) | β a (mV dec−1) | β c (mV dec−1) | CR (mpy) | IE% |
|---|---|---|---|---|---|---|
| Control | −430 | 12.48 | 0.235 | −0.141 | 5.69 | — |
| 0.0005 M | −455 | 5.08 | 0.157 | −0.131 | 2.32 | 60 |
| 0.005 M | −383 | 3.37 | 0.113 | −0.124 | 1.54 | 73 |
| 0.05 M | −368 | 1.87 | 0.379 | −0.059 | 0.85 | 85 |
| 0.2 M | −477 | 2.97 | 0.238 | −0.109 | 1.36 | 76 |