The overall crystallization kinetic parameters of the samples at 115 °C, 120 °C, 125 °C and 130 °C.
| Samples | T c (°C) | t 0.5 (min) | n | k (min−n) |
|---|---|---|---|---|
| PLPG/PDLA-5 | 115 | 2.33 | 2.42 | 6.17 × 10−2 |
| 120 | 2.58 | 2.30 | 1.90 × 10−1 | |
| 125 | 2.98 | 2.02 | 3.19 × 10−1 | |
| 130 | 4.13 | 2.13 | 2.04 × 10−1 | |
| PLPG/PDLA-10 | 115 | 1.63 | 2.53 | 1.37 × 10−1 |
| 120 | 1.80 | 2.10 | 1.38 × 10−1 | |
| 125 | 2.31 | 2.49 | 1.60 × 10−1 | |
| 130 | 2.75 | 2.30 | 1.71 × 10−1 | |
| PLPG/PDLA-15 | 115 | 1.36 | 2.53 | 5.03 × 10−2 |
| 120 | 1.65 | 2.01 | 7.38 × 10−2 | |
| 125 | 1.85 | 2.21 | 1.50 × 10−1 | |
| 130 | 2.76 | 2.29 | 1.46 × 10−1 | |
| PLPG/PDLA-20 | 115 | 1.58 | 2.79 | 1.94 × 10−2 |
| 120 | 1.79 | 2.83 | 4.28 × 10−2 | |
| 125 | 2.03 | 2.13 | 7.49 × 10−2 | |
| 130 | 3.46 | 2.77 | 1.45 × 10−1 |