Melting and crystallization temperatures with their corresponding enthalpy and crystallinity degree for the samples produced (see Table 2 for definition).

Sample code Tm (°C) Tc (°C) ΔHm (J/g) X (%)
rHDPE 127.5 118.1 148.5 51.9
R35 126.6 118.1 94.1 50.6
R50 126.5 118.3 71.2 49.8
R65 127.0 117.8 46.3 46.2
R80 126.7 117.5 26.1 45.6
R15F 127.2 118.0 92.3 49.6
R30F 127.0 117.4 68.6 48.1
R45F 126.0 117.5 47.2 47.2
R60F 126.0 116.8 25.7 44.9
R15F* 127.1 118.6 103.4 52.2
R30F* 126.4 118.5 85.3 50.5
R45F* 127.0 118.3 69.4 49.1
R60F* 126.1 117.8 53.2 48.9

rHDPE: recycled high density polyethylene.