Gas permeability of copolymer and homopolymer membranesa.

Membrane Feed ratio P O2 P CO2 P N2 P O2/PN2 Ref.
SPP : BDPA
Poly(SPP-co-BDPA) 1 : 4 1600 6000 750 2.1 This work
1 : 2 1000 4000 400 2.5
1 : 1 700 3200 250 2.8
2 : 1 650 3000 230 2.8
4 : 1 550 2400 180 3.1
DSpoly(SPP-co-BDPA) 1 : 4 1800 6500 770 2.3
1 : 2 1500 5500 650 2.3
1 : 1 1200 4800 500 2.4
2 : 1 1000 4200 350 2.9
4 : 1 700 3500 200 3.5
SPP : SDPA
Poly(SPP-co-SDPA) 1 : 4 2100 8400 950 2.2 This work
1 : 2 1200 4300 480 2.5
1 : 1 750 3300 280 2.7
2 : 1 700 3000 220 3.2
4 : 1 600 2500 180 3.3
DSpoly(SPP-co-SDPA) 1 : 4 1600 5500 700 2.3
1 : 2 600 2300 170 3.5
1 : 1 380 1600 100 3.8
2 : 1 310 1500 80 3.9
4 : 1 150 1000 38 3.9
Poly(SPP) 240 1300 100 2.4 21 and 22
DSpoly(SPP) 60 310 15 4.0 This work
Poly(BDPA) 1100 4800 500 2.2 10
Poly(SDPA) 1500 4900 680 2.2 11 and 13
DSpoly(SDPA) 900 410 2.2 11 and 13
Matrimid5218 2.12 0.32 6.6 23
Polysulfone 1.4 0.24 5.8 23
6FDA-DAM 55 17 3.3 24
a

Measured at 25 °C, P (barrer), 1 barrer = 10−10 cm3 (STP) cm cm−2 s−1 cmHg−1.