Comments Impact strength/(kJ m−2) Tensile strength/(MPa) Elongation at break/(%) Ref.
PLA/NR-GMA (80/20) 73.4 35 130 160
PLA/SEBS/EGMA (70/20/10) 92 _ 185 164
PLA/PC/SEBS/EGMA (40/40/15/5) >60 _ ∼90
PLA/OBC/EMA-GMA (90/7/3) 64.21 55 ∼30 165
PLA/UFPR (99/1) 2.2 66.26 219.93 198
PLA/NR (95/5) 3.5(2.1) 76.9(84.5) 196.2(16.3) 199
PLA/NR (90/10) _ 40 200 200
PLA/NR/C15A (90/10/1) _ 45 275 202
PLA/NR/C30B (90/10/1) _ 38.2 118 201
PLA/NR (65/35) 58.3 _ _ 205
PLA/NR/DCP (80/20/1.5) 58.3 23 ∼200 206
PLA/NR (60/40) 42.5 ∼22 >100 207
PLA/ENR (60/40) 47 ∼28 ∼150 208
PLA/NBR/DCP (90/9.955/0.045) ∼18 ∼48 >300 249