The textural properties of the RF aerogels synthesized by various Z/R ratiosa.
Z/R | S BET (m2 g−1) | S micro (m2 g−1) | S ext (m2 g−1) | V pore (cm3 g−1) | D pore (nm) | d particle (nm) |
---|---|---|---|---|---|---|
0 | 59.84 | 6.34 | 53.50 | 0.1883 | 102 | 80.1 |
3.24 | 472.31 | 130.43 | 341.88 | 0.7815 | 23 | 12.5 |
6.48 | 487.78 | 172.45 | 315.33 | 0.7096 | 29 | 13.6 |
9.71 | 492.60 | 184.85 | 307.76 | 0.7080 | 33 | 13.9 |
12.94 | 547.96 | 228.28 | 319.68 | 0.7960 | 36 | 13.4 |
The M/R ratio is kept constant as 40.