Comparison of physicochemical data of the copper ion-exchanged samples before and after hydrothermal aging.

Sample name BET surface area (m2 g−1) Micropore volume (cc g−1) Crystallinity (%)
Cu-AC-DABCO 627 0.23 100
Cu-AC-DABCO-700 617 0.23 86
Cu-AC-DABCO-750 616 0.22 75
Cu-AC-DABCO-800 4 0 0
Cu-AC-TEBOP 594 0.20 100
Cu-AC-TEBOP-700 656 0.24 88
Cu-AC-TEBOP-750 679 0.25 86
Cu-AC-TEBOP-800 127 0.04 12
Cu-TR-TEBOP 620 0.22 100
Cu-TR-TEBOP-700 616 0.21 89
Cu-TR-TEBOP-750 579 0.19 88
Cu-TR-TEBOP-800 477 0.16 69