Properties of the papers used in this study.

Properties Paper Paper & primer Paper & primer & pigments & starch Hydrophobized paper & starch
HSI surface treatment (primer) [g m−2] 0 0 ∼0.25 ∼0.25
Pigmentation [g m−2] 0 0 4 0
Surface starch [g m−2] 0 0 ∼1 ∼1
Hydrophobisation (AKD sizing) [kg t−1] 0 0 0 1
Filler content [%] 22 22 23 14
Grammage [g m−2] 97.2 78.5 79.89 77.2
Porosity [%] 40.3 38.8 23.6 20.6
Average pore diameter [μm] 3.9 2.6 3.2 4.9
Roughness [ml s−1] 321 50 78 191.5
Dispersive surface energy [mJ m−2] 44 42 43 33
Polar surface energy [mJ m−2] 27 23 22 0.1
Total surface energy [mJ m−2] 71 65 65 33.1