Degree of conversion (DC), contact angle, water sorption (WS), solubility (SL), and diffusion coefficient (D) of experimental dental resin compositesa.
DC (%) | Contact angle (°) | WS (μg mm−3) | SL (μg mm−3) | D (10−8 cm2 s−1) | |
---|---|---|---|---|---|
TM0 | 62.22 ± 1.98A | 61.6 ± 3.3A | 33.26 ± 3.12A | 8.51 ± 0.39A | 0.92 ± 0.075AC |
TM1 | 61.32 ± 2.14A | 59.2 ± 3.2A | 29.3 ± 5.6A | 7.02 ± 0.28B | 0.82 ± 0.071AB |
TM4 | 59.6 ± 2.15AB | 60.4 ± 4.3A | 26.91 ± 3.99A | 6.72 ± 0.3B | 0.68 ± 0.043B |
TM7 | 56.1 ± 1.17BC | 64.6 ± 4.2A | 42.79 ± 3.56B | 9.82 ± 0.29C | 1.07 ± 0.11C |
TM10 | 54.58 ± 1.64CD | 63.3 ± 4.9A | 46.6 ± 2.32B | 11.52 ± 0.4D | 1.26 ± 0.12D |
Different uppercase letters represent statistically significant differences in same column (P < 0.05).