Skip to main content
. 2018 May 23;8(34):18959–18965. doi: 10.1039/c8ra01963k

Data obtained from pressure–composition isotherms of the Mg–Ni(Fe) sample at various temperatures.

Temperature (K) Low plateau of absorption (MPa) High plateau of absorption (MPa) Maximum hydrogen content (wt%)
598 0.45 0.88 3.0
623 1.41 3.1
648 1.27 1.95 3.6
673 2.05 2.97 3.9