Skip to main content
. 2018 May 29;8(35):19791–19803. doi: 10.1039/c8ra01467a

Glass transition temperature (Tg), crystallization temperature (Tc), melting temperature (Tm) and % crystallinity of drug-loaded mats.

Sample PLA PLA–HCl PLA–base PLA–HCl(DMSO)
T g (°C) 61.1 60.0 60.0 47.1
T c (°C) 89.7 87.9 87.0 86.9
T m (°C) 150.0 150.8 150.0 150.4
Crystallinity (%) 12.9 15.6 16.3 9.4