Comparison of PB molecular parameters prepared via Nd(CF3SO3)3*3TOP and Nd(CF3SO3)3*3TBP systems a.

Run Binary catalyst Temperature (°C) Yield (%) M n × 104e (g mol−1) M w/Mne cis-1,4f (%) trans-1,4f (%) 1,2f (%)
1b Nd(CF3SO3)3 50
2c Nd(CF3SO3)3*3TOP 20 88.2 9.8 1.32 98.8 0.5 0.7
3d Nd(CF3SO3)3*3TOP 50 90.3 10.3 1.46 98.7 0.6 0.7
4c Nd(CF3SO3)3*3TBP 20 83.5 8.7 3.21 98.6 0.5 0.9
5d Nd(CF3SO3)3*3TBP 50 86.9 9.0 3.45 98.6 0.6 0.8
a

Polymerization conditions: solvent is hexane, [Nd] = 8.9 × 10−4 mol L−1, [Al]/[Nd] = 20, [Bd]/[Nd] = 2000.

b

Polymerization time is 24 h.

c

Polymerization time is 2 h.

d

Polymerization time is 30 min.

e

Measured by SEC-MALLS.

f

Measured by FT-IR spectroscopy.