Tensile properties and healing efficiencies of composites C0–5 and BIIR-i.

Sample σ b(v) a [MPa] ε b(v) b [%] H σ c [%] H ε d [%]
BIIR-i 10.2 ± 3.5 960 ± 60 87 ± 50 100 ± 11
C0 12.0 ± 2.3 800 ± 50 40 ± 25 55 ± 19
C1 18.9 ± 2.6 880 ± 40 43 ± 23 71 ± 12
C2 18.9 ± 1.5 970 ± 30 32 ± 16 72 ± 12
C3 10.1 ± 0.7 1030 ± 30 13 ± 8 41 ± 27
C4 11.7 ± 1.5 820 ± 30 n.d.e n.d.e
C5 9.4 ± 0.5 790 ± 20 n.d.e n.d.e
a

Average tensile stress at break of the virgin samples.

b

Average elongation at break of the virgin samples.

c

Healing efficiency related to the tensile stress at break.

d

Healing efficiency related to the elongation at break.

e

Not determined.