Skip to main content
. 2022 May 1;15(9):3256. doi: 10.3390/ma15093256

Table 2.

Thermal changes in A.S. SET 1010 resin samples with 0, 5, 10, 15 and 20 phr cellulose obtained using DSC analysis.

CELLULOSE CONTENT [phr] TEMPERATURE [°C]
ONSET 1 GLASS TRANSITION ONSET 2 PEAK ENDSET
0 56.34 60.42 104.45 136.31 165.88
5 58.04 61.71 109.77 136.96 154.24
10 54.68 58.69 108.35 137.14 165.96
15 63.77 68.32 121.36 134.80 153.81
20 56.34 61.61 104.71 130.12 160.90