Table 2.
Tensile strength and crystallinity of regenerated cellulose fibers with or without additives.
Sample | Tensile Strength (MPa) | Initial Modulus (MPa) | Elongation at Break (%) | Crystallinity (%) |
---|---|---|---|---|
BF | 54.43 ± 2.74 | 382.33 ± 10.66 | 46.8 ± 5.32 | 60.06 ± 2.11 |
UF | 88.57 ± 3.54 | 815.89 ± 9.57 | 33.24 ± 1.79 | 61.58 ± 2.36 |
GF | 105.67 ± 4.50 | 2314.83 ± 26.56 | 13.34 ± 4.38 | 61.89 ± 1.76 |
CCF | 67.29 ± 2.35 | 1323.40 ± 14.89 | 14.35 ± 3.59 | 62.13 ± 1.44 |
CCUF | 117.36 ± 4.28 | 3166.16 ± 30.22 | 13.02 ± 4.31 | 62.50 ± 1.02 |
CCGF | 139.62 ± 5.94 | 3611.72 ± 27.45 | 14.78 ± 2.54 | 62.79 ± 2.00 |