Synthesis of P(St-co-DMAEA) for solubility test via RAFT polymerizationa.
| Run no. | f DMAEA b | Yieldc (%) | F DMAEA d | M n (Mw/Mn)e |
|---|---|---|---|---|
| 1 | 0.10 | 15 | 0.12 | 10 500 (1.07) |
| 2 | 0.20 | 14 | 0.21 | 9900 (1.08) |
| 3 | 0.30 | 20 | 0.29 | 13 600 (1.09) |
| 4 | 0.40 | 8 | 0.36 | 10 200 (1.14) |
| 5 | 0.60 | 21 | 0.48 | 8300 (1.40) |
| 6 | 0.80 | 22 | 0.64 | 6200 (1.55) |
Bulk polymerization; [St + DMAEA]0/[CPADB]0/[AIBN]0 = 500/1/0.2; polym. temp., 60 °C; polym. time, 24 h.
Mole fraction of DMAEA in the feed.
Isolated yield.
Mole fraction of DMAEA unit in the copolymer.
Number average molecular mass and dispersity determined by SEC using polystyrene standards.