Table 3.

DSC data of PLA and PLA-Ag nanocomposites obtained by mechanical and in situ method.

Specimen Glass Transition Cold Crystallization Melting χC, %
Tg,
°C
ΔCp,
J/g·°C
Tccr,
°C
ΔHccr, J/g Tm,
°C
ΔHm, J/g
PLA 59.2 0.412 135.1 16.74 166.1 18.12 19.5
PLA-1 wt.% Ag (mech. method) 61.3 0.378 119.7 37.35 172.3 34.21 37.1
PLA-2 wt.% Ag (mech. method) 61.2 0.432 117.6 34.71 173.2 32.83 36.0
PLA-4 wt.% Ag (mech. method) 60.5 0.443 119.0 35.0 170.9 33.58 37.6
PLA-1 wt.% Ag
(in-situ)
57.6 0.459 112.5 28.5 160/166.4 28.12 32.0
PLA-2 wt.% Ag
(in-situ)
55.7 0.449 103.2 22.97 158.4/165.0 23.51 27.7
PLA-4 wt.% Ag
(in-situ)
54.8 0.394 99.0 20.35 156.5/163.6 25.09 31.9