Skip to main content
. 2022 Jun 10;27(12):3741. doi: 10.3390/molecules27123741

Table 5.

MCC test results of mixtures with kraft cellulose fibres and Tanfloc SG 2.5% + 0.45% A-PAM.

Sample PHRR (W/g) TPHRR (°C) THR (J/g) Char Yield (wt-%)
Bleached SW kraft pulp Test 1
Test 2
Average
315
351
333
380
379
379
11,360
11,550
11,460
6.5
6.6
6.6
Bleached SW kraft pulp + retention aid system Tanfloc SG + A-PAM Test 1
Test 2
Average
361
337
349
372
371
372
12,240
11,870
12,050
6.4
7.5
6.9
+N-modified SW kraft lignin Test 1
Test 2
Average
268
249
258
380
374
377
9520
9120
9320
15.4
14.4
14.9
+N-modified SW CatLignin Test 1
Test 2
Average
265
253
259
380
380
380
9610
9910
9760
14.8
14.5
14.6
+N-modified HW kraft lignin Test 1
Test 2
Average
272
242
257
386
375
381
10,070
9870
9970
14.5
12.9
13.7
+N-modified spruce tannin Test 1
Test 2
Average
247
303
275
371
382
376
9280
10,170
9730
17.8
14.5
16.2