Table 5. Bio-corrosion properties of magnesium-based alloys.
Alloy | Condition | In vitro corrosion rate (mm/year) | In vivo corrosion rate (mm/year) | Reference |
---|---|---|---|---|
Mg-0.8Ca | As-extruded | - | 0.5 | 115 |
Mg-1Ca | As-cast | - | 1.27 | 103 |
Mg-1Al | As-cast | 2.07 | - | 38 |
Mg-1Zn | As-cast | 1.52 | - | 38 |
Mg-1Zn | As-rolled | 0.92 | - | 38 |
Mg-1Zr | As-cast | 2.2 | - | 38 |
Mg-1Zr | As-rolled | 0.91 | - | 38 |
Mg-1Sn | As-cast | 2.45 | - | 38 |
Mg-2Sr | As-rolled | 0.37 | 1.01 | 116 |
Mg-3Zn | Solution treated | 1.53 | - | 100 |
Mg-6Zn | As-extruded | 0.07 | 2.32 | 117 |
Mg-8Y | As-cast | 2.17 | - | 99 |
AZ31 | As-cast | 2 | 1.17 | 39 |
AZ31 | As-extruded | 0.21 | - | 94 |
AZ61 | As-cast | 0.73 | - | 108 |
AZ91D | As-cast | 2.8 | 1.38 | 109 |
WE43 | As-cast | 0.26 | 1.56 | 39, 94 |
Mg-1.2Mn-1Zn | As-cast | - | 0.45 | 36 |
Mg-1Zn-1Ca | As-cast | 2.13 | - | 110 |
Mg-3Zn-0.3Ca | Solution treated | 0.81 | - | 111 |
Mg-6Zn-1Ca | As-cast | 9.21 | - | 110 |
Mg-4Zn-0.5Ca-0.4Mn | As-cast | 0.25 | - | 112 |
Mg-3.09Nd-0.22Zn-0.44Zr | As-extruded | 0.13 | - | 94 |
Mg-2Zn-1.53Y | As-extruded | 0.7 | - | 113 |
Mg-11.3Gd-2.5Zn-0.7Zr | As-extruded | 0.17 | - | 114 |