Sample Furrow Analysis Feature Parameters
Fdmax
(nm)
Fdmean
(nm)
mean
(cm/cm2)
Sda
(µm2)
Sha
(µm2)
Pristine EPI-pBAPS 7.2 3.2 25,878 2.2 0.4
Rubbed EPI-pBAPS (1R) 610.9 234.7 5651 6.4 7.1
Rubbed EPI-pBAPS (2R) 603.9 231.0 5736 14.5 9.6
Rubbed EPI-pBAPS (3R) 497.2 159.5 5287 12.9 12.4
DBD Plasma treated
Rubbed EPI-pBAPS (3R)
534.1 171.7 5820 5.5 3.1
Pristine CBDA-pBAPS 4.4 2.1 21,520 1.3 0.2
Rubbed CBDA-pBAPS (1R) 609.7 180.0 5311 10.7 20.6
Rubbed CBDA-pBAPS (2R) 472.5 136.9 6124 6.1 5.8
Rubbed CBDA-pBAPS (3R) 352.4 87.2 5802 8.1 8.2
DBD Plasma treated
Rubbed CBDA-pBAPS (3R)
368.9 130.9 6407 2.3 1.9

Fdmax: maximum depth of furrow, Fdmean: mean depth of furrow, Fρmean: mean density of furrows, Sda: mean dale area, Sha: mean hill area.