Skip to main content
. 2022 Oct 11;14(20):4258. doi: 10.3390/polym14204258

Table 1.

Compression test results of the first five specimens, compressed at 210 °C and 10 min of dwell time, with various compaction pressures. Appendix D gives the complete results of the experiments including measured standard deviation at each pressure level.

Sample Compaction Press. (MPa) Temp. (°C) Compress. Ratio (%) Loss of Material (%) Density of Comp. Part (g/cm3) Fibre Vol. Fraction (%) Porosity Vol. Fraction (%)
1 10 210 41.09 15.63 1.51 60.99 1.16
2 9 210 38.29 10.07 1.50 61.41 1.06
3 6 210 34.83 5.43 1.49 61.57 1.29
4 4 210 29.85 4.02 1.48 60.43 4.12
5 2 210 29.03 3.21 1.48 59.56 5.45
Preform - - - - - 43.41 8.58