Results of deformation of the test samples between the first and last test cycles in the low-cycle test.

Printing Variant Number of Finished Tests Relative
Deformation 1st Cycle (%)
Relative Deformation 1000th Cycle (%) Strain Difference between 1st and 1000th Cycle (%)
PLA/B/nozzle 0.4 mm/60% 1000 0.069 ± 0.005 0.174 ± 0.005 0.11 ± 0.01
PLA/B/nozzle 0.4 mm/80% 1000 0.072 ± 0.005 0.165 ± 0.014 0.09 ± 0.01
PLA/B/nozzle 0.4 mm/100% 1000 0.065 ± 0.000 0.159 ± 0.016 0.09 ± 0.02
PLA/B/nozzle 0.6 mm/60% 1000 0.069 ± 0.005 0.171 ± 0.011 0.11 ± 0.01
PLA/B/nozzle 0.6 mm/80% 1000 0.072 ± 0.005 0.184 ± 0.005 0.11 ± 0.00
PLA/B/nozzle 0.6 mm/100% 1000 0.078 ± 0.005 0.184 ± 0.005 0.10 ± 0.01