Skip to main content
. 2022 Nov 17;15(22):8166. doi: 10.3390/ma15228166

Table 1.

Summary of the low-temperature electrochemical properties of different notable cathodes.

Material Cell Type Capacity Stability Theoretical Capacity Mass Loading Ref.
LVP/C from KB carbon Half-cell 92 mA·h·g−1
(−30 °C, 4 C)
99% after 500 cycles
(−30 °C, 4 C)
132 mA·h·g−1 1–2 mg·cm−2 [45]
LiFePO4/C Half-cell 109.2 mA·h·g−1
(−20 °C, 0.1 C)
91% after 50 cycles
(0 °C, 0.1 C)
170 mA·h·g−1 N/A [46]
LiFePO4/CNT with conductive network Half-cell 90 mA·h·g−1
(−10 °C, 1 C)
N/A 170 mA·h·g−1 3.7–4.2 mg·cm−2 [47]
LiFePO4/graphene nanofibers Half-cell 124.4 mA·h·g−1
(−20 °C, 0.1 C)
92% after 200 cycles
(−20 °C, 1 C)
170 mA·h·g−1 N/A [48]
LiFePO4/C from fructose and calcium lignosulfonate Half-cell 109.4 mA·h·g−1
(−20 °C, 0.5 C)
N/A 170 mA·h·g−1 N/A [49]
Li2O·B2O3-coated NCM Half-cell 101.9 mA·h·g−1
(−40 °C, 0.2 C)
70.6% after 50 cycles
(−20 °C, 0.2 C)
280 mA·h·g−1 8.2 mg·cm−2 [18]
MnO2-coated LVP/C Half-cell 102 mA·h·g−1
(−20 °C, 1 C)
N/A 197 mA·h·g−1 2.5 mg·cm−2 [50]
CeO2-coated LVP/C Half-cell 103.3 mA·h·g−1
(−20 °C, 1 C)
95.6% after 50 cycles
(−20°C, 5 C)
197 mA·h·g−1 N/A [51]
CeO2-coated LiFePO4/C Half-cell 99.7 mA·h·g−1
(−20 °C, 0.1 C)
N/A 170 mA·h·g−1 N/A [52]
AlF3-coated Li1.2Ni0.13Co0.13Mn0.54O2 Half-cell 109.3 mA·h·g−1
(−20 °C, 0.1 C)
N/A N/A N/A [54]
Polypyrrole-coated LiFePO4 Half-cell 128 mA·h·g−1
(−20 °C, 0.1 C)
N/A 170 mA·h·g−1 N/A [55]
Mo-doped Li1+xNi1/3Co1/3Mn1/3O2 Half-cell 65.4 mA·h·g−1
(−30 °C, 5 C)
N/A 280 mA·h·g−1 N/A [39]
Ti-doped LiFePO4/C Full cell 112.8 mA·h·g−1
(−20 °C, 1 C)
N/A 170 mA·h·g−1 N/A [59]
B-doped Li1.2Mn0.54Ni0.13Co0.13O2 Half-cell 101.9 mA·h·g−1
(−20 °C, 0.2 C)
93.4% after 50 cycles
(− 20 °C, 0.2 C)
N/A N/A [60]
P-doped LiFePO4/C - Half-cell 82.7 mA·h·g−1
(−40 °C, 0.1 C)
N/A 170 mA·h·g−1 1.092 mg·cm−2 [61]
Co-doped Li1.2Ni0.2Mn0.6O2 Half-cell 111.3 mA·h·g−1
(−20 °C, 0.1 C)
58.4% after 40 cycles
(−20 °C, 0.1 C)
N/A N/A [62]
Re-LFP Half-cell 107 mA·h·g−1
(−20 °C, 0.2 C)
N/A 170 mA·h·g−1 N/A [67]
Pure phase LVP Half-cell 90 mA·h·g−1
(−30 °C, 0.2 C)
80% after 1000 cycles
(−10 °C, 10 C)
132 mA·h·g−1 2 mg·cm−2 [68]
Coral-shaped LiFePO4/graphene Full cell 101 mA·h·g−1
(−40 °C, 3 C)
91% after 20 cycles
(−40 °C, 3 C)
170 mA·h·g−1 8–10 mg [69]