Entry Diester R Yielda (%) M calcd (kDa) M n (GPC) (kDa) M w/Mnb Trans contentc (%) T g (°C) T 5d (°C)
1 7 Me 68 3.6 7.11 1.08 53 121 231
2 8 Et 62 3.9 5.96 1.07 51 114 235
3 9 n Pr 58 4.0 5.07 1.05 47 107 236
4 10 iPr 57 4.1 4.89 1.09 45 109 182
5 11 n Bu 49 4.3 2.73 1.09 45 96 162
a

Isolated yield after precipitation.

b

Values of Mw/Mn determined by GPC with polystyrene standards.

c

Determined by 1H NMR.

d

Temperature at 5% weight loss.