Abstract

The performance of biomaterials in biological systems is of critical significance for advancing biomedical implants. Duplex Stainless Steel alloys are the major biomaterials due to their significant characteristics. Many functional coatings are deposited on DSS alloy surfaces utilizing numerous surface coating techniques to improve their bioactivity and protect them from corrosion degradations. Coatings of titanium dioxide (TiO2), Hydroxyapatite (HA), and zinc oxide (ZnO) have received considerable attention in the field of surface bioactive modification of DSS alloy implants. The coating techniques play a key role in increasing the required biological characteristics of DSS alloys, such as biocompatibility, mechanical properties, and corrosion resistance. In this regard, HA-ZnO, HA-TiO2, and TiO2–ZnO from each coating group are divided into single, double, and triple layers. These coatings were prepared by cold spray and deposited on the surface of the DSS alloy, followed by a heat treatment at 250 °C. The surface morphology of coated surfaces was analyzed utilizing field emission scanning electron microscopy (FESEM), atomic force microscopic (AFM), microhardness test, corrosion test in Ringer solution, and antibacterial test. The coatings showed nano-scale surface morphology with advanced crystallization and homogeneous structures; in the corrosion characteristics utilizing potentiodynamic polarization, triple layers of HA-ZnO coatings displayed advanced nanostructures with higher hardness values (514.75HV). The antibacterial test showed the triple layers of HA-TiO2 and two layers of TiO2–ZnO sensitivity to positive bacteria.

Keywords: Surface modification, Hydroxyapatite, Titanium dioxide, Zinc oxide, Biomedical, Cold spraying

1. Introduction

"Biomaterials" refers to nonviable materials designed to interact with biological systems to assess, treat, enhance, or substitute any tissue, organ, or bodily function [1]. A new biomaterial's mechanical, functional tissue pathobiology and structure designated anatomic location, as well as other property regulation, standardization, ethics, the healing process, biocompatibility, toxicology, and requirements, are all taken into account before it is released onto the market [2,3]. In order to meet the needs of aging populations and prolong human life while improving quality of life, the area of biomaterials has shown fast structural and characteristic improvement [4,5]. Functional coatings applied to the surface of metal implants are a major way to increase their bioactivity and protect them from severe degradations like corrosion and wear [6].

A biomaterial must meet the crucial condition of being biocompatible. When utilized in a particular application, a biocompatible material responds to the host appropriately (i.e., there is little disturbance of normal bodily function) [7]. Therefore, when utilized in vivo, the substance does not result in a thrombogenic, toxic, or allergic inflammatory reaction. The host responses that a material causes and the degradation of the substance in the bodily environment are the two main determinants of a material's biocompatibility. Both elements should often be taken into account [8].

The selection and design of alloys and metals for usage in vivo must consider corrosion. Throughout corrosion processes, allergenic, toxic/cytotoxic, or carcinogenic compounds (such as Al, V, Cr, Co, or Ni) might be released into the body. Additionally, several corrosion processes may cause implant failure and loosening [9,10]. As a result, corrosion and solubility tests are often necessary before biomaterials are certified by regulatory entities. So, in the context of quality control, implant retrieval analysis, and failure analysis, the corrosion behavior of metal implants was thus extensively researched.

The outermost atomic layer or outside limit of the substance. A surface's shell enclosing an item from its surroundings is another definition of the word surface. The interface is the area at the border between two neighboring phases, even between a liquid and a solid. Since they will be in touch with the host molecules and atoms or their immediate surroundings, the atoms and molecules making up the surface will control the surface characteristics of that substance. Because there are fewer dangling bonds in bulk materials than in microscopic particles of the same volume, the surfaces of these materials vary. Chemical connections called dangling bonds are connected to atoms on the surface of solids. Surface atoms extend in the direction of the outside of the solid or in the direction of the vacuum. Still, they do not unite an atomic with a second atomic from their exterior side [11].

Additionally, surface modification is the adsorption of different ligands or molecules to produce certain biological, chemical, or physical characteristics. Surface modification may be accomplished by physically or chemically altering the atoms or molecules on the surface or by covering the surface with a layer. The layer might be organic, a polymer layer, or a thin film made of another substance. In order to increase the interfacial qualities of a material, including wettability, the adsorption of ligands and proteins, and enhanced roughness, surface modification is utilized [12]—Fig. 1 displays many surface alteration techniques. Various techniques may be utilized depending on the substrate's surface and the desired level of alteration.

Fig. 1.

Fig. 1

The schematic diagram for coatings categorization.

An object's surface is coated to improve its surface attributes, including electrical conductivity, dielectric property, wettability, adhesion, scratch resistance, wear resistance, corrosion resistance, appearance, etc., or to protect it from environmental impacts. The term "substrate" might even refer to the item that will be coated. In certain circumstances, the coatings serve as a crucial component of the end product, like in the manufacture of semiconductor devices utilizing a silicon wafer as the substrate. Individuals might apply coatings as liquids, gases, or solids. Spray coating is the term for a coating that is applied to an item utilizing a liquid spray. The most recent emerging coating techniques are suspension and solution thermal spraying [13]. Thermal energy is utilized in the thermal spraying process to melt material in powder, wire, or rods. The process gases are expanded to provide kinetic momentum to drive the molten or semi-molten material toward a prepared surface. A coating accumulation known as spray coating results from the impact of these molten or semi-molten particles on the surface of the substrate.

Since thermal energy has not been utilized as the major energy source, cold spray is not strictly a thermal spray process. In cold spraying, the carrier gas is driven thru a converging-diverging de Laval-type nozzle, accelerating particles to very high speeds. When a solid feedstock particle strikes a substrate with much energy, the particles near the surface deform plastically and then metallurgically attach to the substrate to produce a coating. The essential velocity magnitude for bonding relies on the material parameters, including the kind of feedstock, the size of the powder, and the temp. Velocity is a crucial factor in coating production. Although certain hard materials have also been observed, soft metals like Al and Cu work well for cold spraying [14].

Several techniques have been employed to deposit coating layers on the surfaces of metallic materials, such as coating by vacuum spin coater device. Currently, there are several kinds of engineering materials utilized as implantable materials. Among these biomaterials, metallic materials are the most utilized in implant applications. In this regard, Duplex Stainless Steel is the major bio-metallic material. Therefore, there is crucial to increase the implant lifespan to promote good integration and bonding with surrounding bone [15,16]. Because its metallurgical structure comprises two phases, ferrite (body-centered cubic lattice) and austenite (face-centered cubic lattice), in about equal amounts, duplex stainless steel (DSS) grades are also known as austenitic-ferritic grades [17]. Specialized "hyper-duplex" grades, Super grades, Regular grades, and Lean grades are the categories into which DSS has developed [18]. Since the synergistic impact of high molybdenum and nitrogen amounts, the DSS possesses localized resistance to corrosion that is as excellent as titanium alloys. It has excellent mechanical qualities as well. The literature demonstrates that austenitic-ferritic and austenitic steels have comparable biocompatibility. Austenitic-ferritic steel decreases expenses and patient nickel hypersensitivity in orthodontic procedures when austenitic stainless steel is replaced [18]. Utilizing potentiodynamic measurements and electrochemical impedance spectroscopy (EIS), Kocijan et al. [19] investigated the development of the passive layer on AISI 316 L stainless steel and DSS in artificial saliva with the adding fluoride. For both solutions, the DSS's passive range was larger than it was for the AISI 316L. While the Fe species have been noticeably reduced, Cr-oxides predominated in the passive layer on both materials. In order to assess the suitability of duplex stainless steel as a biocompatible material, Gregorutti et al. [20] examined its magnetic, electrochemical, and mechanical characteristics. They contrasted the outcomes with those of austenitic stainless steel. DSS has roughly two times higher yield and ultimate tensile strengths. According to the electrochemical test, this material is less susceptible to localized corrosion.

The impact of clean production (green production) techniques on the duplex stainless steel's surface morphology were examined by Krolczyk et al. [21]. Power Spectral Density was utilized to compare the surface quality between the dry and MQCL turning processes. Analysis of the surface's signal power showed that dry turning had a longer wavelength than machining utilizing the MQCL process. At lower feed rates, tool vibration is dominated by the cutting tool wear tip and is noticeable in the feed ingredient's amplitude ranges. By comparing this function's qualitative and quantitative results for the examined surfaces, the research researchers demonstrated that it is feasible to define turning about applied cooling techniques utilizing PSD. Furthermore, for various feed levels, the amplitudes of the investigated surfaces range roughly from 1.81 m to 2.10 m.

Surface integrity (SI) microhardness was observed by Krolczyk et al. [22]. After turning with coated sintered carbide wedges, surface integrity (SI) microhardness was observed. SI is crucial in both the beginning of fatigue cracks and corrosion resistance. Microhardness evaluations of DSS during dry and wet machining were part of the project. We compared SI's microhardness at different cutting rates. It was demonstrated that cutting with water reduces the SI hardening depth; however, expanding the wedge's rounded cutting edge radius raises both the maximal microhardness magnitudes and the hardening depth. The rounded cutting-edge radius has been investigated utilizing an infinite focus measuring device. The investigation was conducted in a manufacturing environment that produced sheets with explosive cladding, deep-well pumps, and electric motor components.

In order to repair or refurbish pharmaceutical components, Ralls et al. [23] examined the corrosion and wear behavior of high-pressure cold-sprayed (CS) 316 L stainless steel (SS) and compared it to conventional 316 L SS. The CS deposit has been found to have a compact microstructure with a higher proportion of the ferrite phase. Because of localized adiabatic heating and pressures from the highly deformed particles, the action of CS also caused a refinement of crystallinity. As a result of these impacts, the CS deposit showed less abrasive wear, which resulted in less friction and wear. Electrochemical experiments also showed that the CS specimen had a better capacity to re-passivate while exhibiting a roughly comparable corrosion rate to the bulk specimen.

On duplex stainless steel substrates, pure nickel (Ni) and nickel-Inconel 718 powder deposits were created utilizing the cold spray approach by Kazasidis et al. [24]. In order to create high-quality coatings, nitrogen was utilized as the propellant gas. Because of the extremely ductile binder phase required for manufacturing, the coatings demonstrated good Inconel 718 (In718) retention inside the Ni matrix. Microhardness, energy-dispersive X-ray spectroscopy, electron microscopy, and X-ray diffraction tests characterize the coating microstructures. Additionally, cavitation erosion experiments were utilized to assess the resistance to erosion of both coatings, and a study of the eroded surfaces revealed various erosion processes for every coating. The findings showed the effectiveness of the cold spray method for producing coatings for metal-metal matrix composites and the potential of In718 for usage in situations requiring increased cavitation erosion resistance.

TiO2, in the form of nanocrystals, contains photocatalyst capabilities, which leads to a great capacity for degrading various environmental pollutants, including viruses, bacteria, and organics. Nevertheless, the antibacterial activity of nano-TiO2 coatings against various diverse microbes has yet to be confirmed to be a high level of reliability. Common nosocomial and environmental microorganisms such as Streptococcus mutants, Staphylococcus aureus, Aspergillus niger, and Candida albicans are responsible for biofilm-associated infections, particularly indoors [[25], [26], [27]]. Since the widespread application of titanium dioxide (TiO2) and zinc oxide (ZnO) nanoparticles in sunscreens and cosmetics, a significant amount of research has been conducted on metal oxide nanoparticles in the field of toxicology [28]. Several of these studies have focused on zinc oxide (ZnO) and titanium dioxide (TiO2) nanoparticles [25]. ZnO and TiO2 nanoparticles do not permeate the skin, as was noted in a recent review [28,29]; as a result, it has been suggested that they do not constitute possible harm to human health once placed onto the skin that has not been injured [30]. Nevertheless, due to the semiconducting qualities of ZnO nanoparticles, industrial and electrical applications have received much interest, along with new potential routes of exposure and dangers.

Researchers have studied the inflammatory impacts of ZnO and TiO2 nanoparticles in vivo [31] and in vitro [32], but researchers still need to comprehend how nanoparticles impact the human immune system fully. The majority of information comes from research on cell lines that is repeatable and well-standardized tests. Uncertainty exists on how well these findings apply to basic human cells. The impact of nanoparticles on human peripheral blood mononuclear cells (PBMC) has only been investigated in a small number of research [[33], [34], [35]]. The simultaneous analysis of the impacts of nanoparticles on several distinct critical immune cells, including natural killer (NK) cells, monocytes, B-cell, and T-cells, is made possible using PBMC. As a result, monocytes had particular impacts when PBMC were exposed to silver nanoparticles, although T-cell proliferation was unaffected [35]. The antigen-presenting cells (APCs) in the body with the strongest potential to trigger and guide immune responses and the highest likelihood of coming into contact with and taking up nanoparticles in vivo are dendritic cells (DC). An established technique is to produce monocyte-derived dendritic cells (MDDC) for in vitro investigations because they are so few in peripheral blood, less than 1% [36].

The form in which hydroxyapatite (HAp) manifests itself in biological systems is distinct from the manner in which it is created as an assortment of calcium phosphates. Hydroxyapatite is a complex ceramic substance [[37], [38], [39]]. HAp differs in the electrical polarization, grain size, and crystallinity of its grains, as well as the chemical composition of its replacing atoms. HAp can form solid, macro, micro, and nanoporous structures. Additionally, particle HAp may have a very permeable structure. Coatings made of HAp may be applied on metal implants, ranging in thickness from hundreds of microns to hundreds of nanometers, depending on the desired application. Infections that occur after implantation are regarded as one of the most difficult problems to solve in medicine, which is why researchers are always working to produce bactericidal functional coatings. The synergistic combination of zinc oxide (ZnO) and hydroxyapatite (HAp) has favorable features, such as good bioactivity, which is further enhanced by the fact that ZnO is antimicrobial. The electrophoretic deposition was used by Geuli et al. [40] in order to manufacture extremely phase-tunable pure ZnO-HAp nanocomposite coatings. Separate batches of HAp and ZnO nanoparticles were produced, concurrently dispersed, and then electrophoretically placed onto a titanium substrate. By adjusting the potentials at which the ZnO-HAp was deposited, it was possible to produce a single-stage graded coating of the material. In addition, we could accurately create composite coatings with a predetermined phase ratio between ZnO and HAp by regulating the content of the nanomaterials in the dispersions, which was accomplished by managing the composition of the nanomaterials. In vitro studies, antibacterial [41,42], cytotoxicity, and bioactivity tests demonstrated superior performance by increasing the mineralization of the coating, improving cell proliferation, and successfully eradicating E. coli bacteria. These benefits were achieved even though the tests were conducted in a laboratory setting.

The current research aims to investigate the advancement of Duplex Stainless Steel (DSS) alloy bioactivity and protect them from corrosion degradations; large kinds of functional coatings are deposited on DSS alloy surfaces utilizing cold spray coating. Also, improved biocompatibility, mechanical and corrosion resistance properties for DSS by applying HA-ZnO, HA-TiO2, and TiO2–ZnO coatings deposited on the surface of DSS alloys system by cold spray device followed by a heat treatment at 250 °C.

2. Experimental work

2.1. Substrate preparation

An alloy of 2507 DSS made in Sweden's Outokumpu factory for stainless steel and high-performance alloys. The chemical composition of this alloy is shown in Table .1. The first step is grinding specimens by grinding sheets (400) and then ultrasonically cleaning ultrasonic cleaner for 10 min with ethanol.

Table 1.

Chemical composition (wt.%) analysis of the used 2507 DSS.

Alloy UNS Cr Ni Mo C N Fe
2507 S31050 25.59 7.03 4 0.017 0.311 balance

2.2. Preparation of coating solutions

Three coating solutions are prepared according to the following concentrations and materials; First solution; 0.9 g H A, 0.05 g ZnO, and 100 ml ethanol; second solution; 0.9 g H A, 0.05 g TiO2 and 100 ml ethanol; third solution; 0.05g ZnO, 0.05 g TiO2 and 100 ml ethanol. Each solution is stirred by a stirrer for 15 min continuously and then mixed for 10 min with an ultrasonic mixing liquid. The coating process was accomplished by a vacuum spin coating device (Fig. 2); throughout the spin coating, a low amount of the solution is dropped on the substrate spun by the spin coater under a high centrifugal force, resulting in the solution being uniformly distributed over the substrate. Then put the samples in the oven at 250° centigrade for 1 h, after which extract the samples from the furnace. The process of coating a second layer on the second and third samples and putting them in the furnace at 250-degree centigrade for 1 h and then extracting them and the process of coating the third layer on the third sample and putting them in the furnace at 250-degree centigrade for 1 h and then extract, the samples were cooled slowly to room temperature.

Fig. 2.

Fig. 2

Vacuum spin coater device.

2.3. Spin coating method

Spin coating is a method for evenly dispersing thin coatings over flat surfaces. Typically, a small quantity of coating material was deposited to the substrate's core, either not spinning at all or rotating at a low speed. The coating material was disseminated by centrifugal force while the substrate spun at speeds up to 10,000 rpm. Spin coaters, or merely spinners, are devices utilized for spin coating. Rotation is maintained until the appropriate film thickness is reached, whereas the fluid spins off the substrate's edges.

2.4. Characterization tests

2.4.1. Field emission scanning electron microscopy (FESEM)

The FESEM micrographs are shown for the as-prepared sample; FESEM images exhibit the surface morphology and the distribution of nanoparticles. Field Emission Scanning Electron Microscopy test is used to identify microstructural features and performed using FESEM kind (MIRA 3-XMU), University of Tehran.

2.4.2. Atomic force microscopy (AFM)

Atomic force microscopy creates a three-dimensional image of the sample surface with high magnification; AFM is utilized to study of size, shape, and aggregation of inner particles. The surface image feature, particle size, and nano roughness of the deposition layer are observed with the atomic force microscope (AFM) using AFM (SPM AA3000, Angstrom Advanced Inc., USA).

2.4.3. Hardness test

Vickers Hardness (TH715, Digital Micro Vickers Hardness Tester). It was utilized to measure the hardness of the coating at a load (300g) and a holding time of 15 s according to ASTM (E384 M) standard.

2.4.4. Antibacterial test

The antibacterial effect of coated DSS alloys with the solutions mentioned earlier is investigated against bacteria Staphylococcus and E coil. The antibacterial activity of the surface layer of modified Duplex Stainless Steel was investigated. The activity of antibacterial is studied by using the inhibition zone method. An antibacterial kinetic test with bacterial strains of "E.coli" (Escherichia coli, American type culture, "ATCC 25922″, gram-negative bacteria, is prepared at the laboratory. The E.coli grown on an (N. agar) "nutrient agar" and placed in the incubator for 24 h, then the bacteria spread on a Petri dish and incubated at 37 °C for 24 h; after that, the samples were placed in four different regions on the Petri dish, and the inhibition zones are observed.

2.4.5. Electrochemical test

After surface modifications, the electrochemical corrosion tests were studied for the samples by polarization tests (potentiodynamic). These tests are done in "Ringer's solution" (chemical composition detailed in Table 2). This test is performed by utilizing potentiostats/galvanostats (MLab Bank Elektronik, Germany, at the University of Babylon– Department of Metallurgical Engineering. There are three electrodes in the corrosion cell:

  • 1.

    The electrode of the working "coating sample."

  • 2.

    The counter electrode (platinum rod).

  • 3.

    The saturated calomel electrode (SCE).

Table 2.

"Ringer's solution" Chemical Ingredients.

Component Concentration (g/L)
NaCl 8.60
KCl 0.30
CaCl2.2H2O 0.33
pH 5–7.5

The exposed surface area was (1.767 cm2) for the electrode working used for all samples.

The following equation is used to calculate the corrosion rate [43]:

CR(mpy)=0.13icorr(E.W.)/A.ρ (1)

E. W. = equivalent weight (g/eq).

A = area (cm2)

ρ=density (g/cm3)

0.13 = metric and time conversion factor

Icorr. = current density (μA/cm2)

The improvement % was computed for specimens with coating using the following equation (2):

improvementpercentage(CR0−CR/CR0)×100 (2)

Where:

CR° = the corrosion rate of the main specimen (without coated)

CR = the corrosion rate of the coated specimen (with coated)

3. Results and discussion

3.1. FESEM results

In the case of a single layer of ZnO-HA coating, nanoparticles appear with a mean particle size of about 36.16 nm (Fig. 3A). In the case of double layers of ZnO-HA coating, nanoparticles appear with a mean particle size of about 61.47 nm (Fig. 3B). In the case of a triple layer of ZnO-HA coating, nanoparticles appear with a mean particle size of about 92.83 nm (Fig. 3C), notice in (Fig. 3B) that the homogeneity of the coating is better and its spread over the surface is.

Fig. 3.

Fig. 3

FESEM for HA-ZnO coating.

Through the use of cross-sectional SEM images, we were able to investigate the overall coated specimens. Images of sectioned, as-deposited cold spray coatings on clean substrates are shown in Fig. 3 (A, B, and C). These coatings were created with three different numbers of coating layers. The coatings had a thickness that varied from 78 m to 123 m over their surfaces. Image examination of the cross-sectional pictures showed that the amount of porosity dropped as the number of coating layers increased, and this was found to be the case. In the SEM pictures, the interface between the coatings and the substrates was difficult to detect, which is evidence of the strong connection between the coating and the substrate. Differences in grain structure between the coatings and the substrates were the sole thing that allowed for the identification of the interface. It is anticipated that the close contact would result in high levels of adhesion strength [44].

In the case of a single layer of TiO2-HA coating, nanoparticles appear with the mean particle size of 58.33 nm (Fig. 4A); in the case of double layers of TiO2-HA coating, nanoparticles appear with a mean particle size of approximately 97.71 nm (Fig. 4B). In the case of a triple layer of TiO2-HA coating, nanoparticles appear with a mean particle size of 32.66 nm (Fig. 4C). In the case of a single layer of ZnO–TiO2 coating, nanoparticles appear with a mean particle size of 64.43 nm (Fig. 5A). In the case of double layers of ZnO–TiO2 coating, nanoparticles appear with the mean particle size of 48.96 nm (Fig. 5B); in the case of a triple layer of ZnO–TiO2 coating, nanoparticles appear with a mean particle size of approximately 60.62 nm (Fig. 5C).

Fig. 4.

Fig. 4

FESEM for HA-TiO2 coating.

Fig. 5.

Fig. 5

FESEM for ZnO–TiO2 coating.

3.2. Atomic force microscopy (AFM) results

The AFM analysis is done for them; HA-ZnO, HA-TiO2, and TiO2–ZnO from each group of these coatings are divided into single, double, and triple layers. The topography of the deposited sample and particle distribution in the deposited layer with a 3D performance image is shown in Fig. 6, Fig. 7, Fig. 8, Fig. 9, Fig. 10, Fig. 11, Fig. 12, Fig. 13, Fig. 14. The different particle distributions for the mentioned samples are shown in Figures B (6–14). It appears that the granularity accumulations for the deposition layer with an average diameter in this condition are shown in Table 3

Fig. 6.

Fig. 6

a) 3-D topographic images for HA-ZnO (single layer) surface roughness: b) histograms of the height distribution of the sample (HA-ZnO (single layer)).

Fig. 7.

Fig. 7

a) 3-D topographic images for HA-ZnO (double layers) surface roughness; b) histograms of the height distribution of the sample (HA-ZnO (double layer)).

Fig. 8.

Fig. 8

a) 3-D topographic images for HA-ZnO (triple layer) surface roughness; b) histograms of the height distribution of the sample (HA-ZnO (triple layer)).

Fig. 9.

Fig. 9

a) 3-D topographic images for HA-TiO2 (single layer) surface roughness; b) histograms of the height distribution of the sample (HA-TiO2 (single layer)).

Fig. 10.

Fig. 10

a) 3-D topographic images for HA-TiO2 (double layer) surface roughness; b) histograms of the height distribution of the sample (HA-TiO2 (double layer)).

Fig. 11.

Fig. 11

a) 3-D topographic images for HA-TiO2 (triple layer) surface roughness; b) histograms of the height distribution of the sample (HA-TiO2 (triple layers)).

Fig. 12.

Fig. 12

a) 3-D topographic images for ZnO–TiO2 (single layer) surface roughness; b) histograms of the height distribution of the sample (ZnO–TiO2 (single layer)).

Fig. 13.

Fig. 13

a) 3-D topographic images for ZnO–TiO2 (double layer) surface roughness; b) histograms of the height distribution of the sample (ZnO–TiO2 (double layers)).

Fig. 14.

Fig. 14

a) 3-D topographic images for ZnO–TiO2 (triple layer) surface roughness; b) histograms of the height distribution of the sample (ZnO–TiO2 (triple layers)).

Table 3.

Average values of particle size and surface roughness by AFM analysis.

Samples Average Thickness (nm) Average Roughness (nm)
ZnO-HA single layer 78.0671 14.2707
ZnO-HA double layers 123.172 14.8572
ZnO-HA triple layers 119.146 25.6925
HA-TiO2 single layer 57.1869 15.0603
HA-TiO2 double layers 217.958 26.282
HA-TiO2 triple layers 100.388 17.4578
ZnO–TiO2 single layer 25.5226 5.92
ZnO–TiO2 double layers 100.098 20.4597
ZnO–TiO2 triple layers 64.8645 12.3675

In the case of a single layer sample of ZnO-HA coating has average roughness (Ra = 14.2707 nm) (Fig. 6 a & b), in the case of double layers sample of ZnO-HA coating has average roughness (Ra = 14.8572 nm), (Fig. 7 a & b). In the case of a three layers sample of ZnO-HA coating has average roughness (Ra = 25.6925 nm) (Fig. 8 a & b) [45].

Fig. 6, Fig. 7, Fig. 8 show results from atomic force microscopy AFM of ZnO-HA single layer, double layers and triple layers coating deposited, it can be noticed that average roughness of deposited layers are affected by increasing the number of layers. It can be seen that the coating thickness increased with the number of layers increasing.

In the case of a single layer sample of TiO2-HA coating has average roughness (Ra = 15.0603 nm) (Fig. 9 a & b), in the case of double l layers' sample of TiO2-HA coating has average roughness (Ra = 26.282 nm) (Fig. 10 a & b). A triple-layer sample of TiO2-HA coating has average roughness (Ra = 17.4578 nm) (Fig. 11 a & b). Fig. 9, Fig. 10, Fig. 11 show the results from the atomic force microscopy of HA-TiO2 composite multi layers coating. Here, it notes that the surface was smoother when a single layer was used and after that, the surface roughness continued to increase with an increase in the number of layers until it reached the roughest surface when the triple layers.

A single-layer sample of TiO2–ZnO coating has average roughness (Ra = 5.92 nm) (Fig. 12 a & b). Due to the utilized ZnO–TiO2 materials nanoparticles size between 20 and 30 nm, the deposition layer was a single layer with 25.5226 nm; therefore, the surface roughness obtained from taking the average value between upper and lower peaks for the deposited layer shows no significant variance; therefore the roughness is low value. In the case of double layers' the sample of TiO2–ZnO coating has average roughness (Ra = 20.4597 nm) (Fig. 13 a & b). A triple layers sample of TiO2–ZnO coating has average roughness (Ra = 12.3675 nm) (Fig. 14 a & b).

Fig. 12, Fig. 13, Fig. 14 show results from atomic force microscopy AFM of ZnO–TiO2 single layer, double layers and triple layers coating deposited, it can be noticed that average roughness of deposited layers are affected by increasing the number of layers. It can be seen that the coating thickness increased with the number of layers increasing.

3.3. Hardness results

The results of the micro-hardness of samples coated by HA-TiO2, HA-ZnO, and TiO2 -ZnO are demonstrated in Fig. 15. It could be observed from Fig. 15 that the hardness of the sample coated with triple layers of HA-ZnO was (514.75 HV), which is higher than the hardness of the sample coated with double layers of HA-ZnO (364 HV), and the hardness of the sample coated with a single layer of HA-ZnO (306.6 HV). The hardness of the sample coated with triple layers of HA-TiO2 was (382.04 HV), which is higher than the hardness of the sample coated with double layers of HA-TiO2 (396.64 HV), and the hardness of the sample coated with a single layer of HA-TiO2 (361.67 HV). The hardness of the sample coated with triple layers of ZnO–TiO2 was (477.73 HV), which is higher than the hardness of the sample coated with double layers of ZnO–TiO2 (448.87 HV) and the hardness of the sample coated with a single layer of ZnO–TiO2 (420.45 HV). The morphology and microstructure of the surface coating also have a significant impact on the surface hardness magnitudes. The final bioactive HA coating's interface and bonding strength with the surface of the DSS alloy substrate was significantly improved by the nanoscale intermediate TiO2 layer [46]. The standard deviation for the hardness value is 76.69712, while the improvement percentage for the selected coating ranges from 17% to 96%. Therefore, the sample HA-ZnO-3 layer gains the highest hardness value compared with other coating layers due to increasing the thickness of the deposited layers that result from increasing the layer number.

Fig. 15.

Fig. 15

Hardness results.

3.4. Antibacterial test results

A bacterial sensitivity test to the substances in question was conducted, and the result was as follows:

First: E.coil, a gram-negative bacteria, showed resistance to all samples from (ZnO-HA single layer, ZnO-HA double layers, ZnO-HA triple layers, HA-TiO2 single layer, and HA-TiO2 double layers with ZnO–TiO2 triple layers), due to its possession of resistance factors to these substances as shown in Fig. 16.

Fig. 16.

Fig. 16

Antibacterial results.

Second: As for staphylococcus aureus, which is a gram-positive bacterium, it showed resistance to substances from samples (ZnO-HA single layer, ZnO-HA double layers, ZnO-HA triple layers, HA-TiO2 single layer, and HA-TiO2 double layers as well as ZnO–TiO2 triple layers). As for samples (HA-TiO2 triple layers, ZnO–TiO2 single layer, and ZnO–TiO2 double layers), it showed its effect or sensitivity to these substances because these substances have an anti-wall effect, as shown in Fig. 17. The cell walls or the plasma membrane of the bacterial cell wall may affect the DNA, genetic material of bacteria, or some intermediate processes of enzymatic reactions [25,41,[46], [47], [48]].

Fig. 17.

Fig. 17

Antibacterial results.

3.5. Potentiodynamic polarization

Table (4) shows the potentiodynamic polarization curves for base DSS substrate and coating samples in the Ringer's solution at 37 °C for a different time. The corrosion current (icorr) and corrosion potentials (Ecorr) are derived from the potentiodynamic curves using Tafel extrapolation. In addition, the corrosion rates (CR) were also included in this table and estimated by Equations (1), (2).

Investigation of corrosion behavior of uncoating DSS and coating samples was obtained by potentiodynamic polarization test. At first, the sample is immersed in Ringer's physiological solution for 30 min. The open circuit potential (OCP) has been recorded after this period, where a steady state potential is attained. The corrosion behavior has been studied for different samples (see Table 4).

Table 4.

Hardness value and improvement percentage.

Sample ID Hardness value HV Improvement percent
Uncoated 262 261
HA-ZnO-1 layer 306.6 17.02%
HA-ZnO-2 layer 364 38.93%
HA-ZnO-3 layer 514.75 96.47%
HA-Ti2O-1 layer 361.67 38.04%
HA-Ti2O-2 layer 369.64 41.08%
HA-Ti2O-3 layer 382.04 45.82%
ZnO–Ti2O-1 layer 420.45 60.48%
ZnO–Ti2O-2 layer 448.87 71.32%
ZnO–Ti2O-3 layer 477.73 82.34%
Standard deviation 76.69712

The coating of (a single layer) has the lowest corrosion rate than the uncoated sample, (and triple layers) have a low corrosion rate than double and single layers. The samples with single or double layers result in an incomplete coating scale that produces a nonhomogeneous layer. Moreover, the porosity in the microstructure allows the corrosive fluid's penetrability into the substrate and corrodes it as shown in Table 5.

Table 5.

The corrosion rate of the coated substrates with HA-TiO2, HA-ZnO, and TiO2–ZnO.

Samples icorr (μA) Ecorr (mV) C.R (mpy) Improvement %
2507 DSS without coating 22.400 26.7 2.786 –
ZnO-HA single layer 14.450 −57.4 0.419 85
ZnO-HA double layers 2.603 −123.3 0.075 97
ZnO-HA triple layers 0.04284 −304.8 0.011 99
HA-TiO2 single layer 1.200 −159.0 0.326 88
HA-TiO2 double layers 0.99038 −105.6 0.269 90
HA-TiO2 triple layers 0.50153 −298.2 0.136 95
ZnO–TiO2 single layer 0.06545 85.9 0.027 99
ZnO–TiO2 double layers 0.05271 −69.7 0.022 99.2
ZnO–TiO2 triple layers 0.03922 −21.0 0.016 99.5

The results disclose that substrates coated with triple layers exhibit nobler values than those coated with double or single layers. Since the extraordinary protective nature of coated layers versus corrosion assaults, the coated materials with HA-TiO2, HA-ZnO, and TiO2–ZnO significantly boost corrosion resistance.

The sample coated with triple layers of TiO2–ZnO has the best corrosion resistance, as well as excellent corrosion behavior of triple, double and single layers coating of TiO2–ZnO could be attributed to its uniform, dense, and compact surface structure and outstanding adhesion strength film into DSS alloy surface, compared with the other type of coating HA-TiO2 and ZnO-HA. Moreover, the thickness values of triple and double layers of the coating were measured to be more than that of the single layer. The coating layers offer improved anticorrosion characteristics for DSS alloy under the difficult situations of the physiological solution [46,49], as shown in Fig. 18a-i. As well as, increased corrosion resistance leads to increased antibacterial resistance due to the absence of physiological media leaking out to the substrate.

Fig. 18.

Fig. 18

Polarization diagrams for a) HA-ZnO (single layer); b) HA-ZnO (double layers); c) HA-ZnO (triple layer) HA-TiO2; d) HA-TiO2 (single layer); e) HA-TiO2 (double layer); f) HA-TiO2 (triple layer); g) ZnO–TiO2 (single layer); h) ZnO–TiO2 (double layers); i) ZnO–TiO2 (triple layers).

4. Conclusions

In this paper, prepared and investigated three various coatings with single, double and triple layers of each HA-TiO2, HA-ZnO, and TiO2–ZnO were successfully deposited on the surface of (2507) DSS alloys by vacuum spin coating devices for biomedical applications. These bio-coatings were described concerning surface topography, micro-hardness, activity against bacteria, and corrosion. The conclusions of this investigation can be drawn as following:

  • •

    Layer coating is composed of nanoscale granular-like particles and regular micro and nano pores in a compact structure with better homogeneity and much smaller dimensions that are not damaged, cracked, or disintegrated.

  • •

    Samples with high number of layers coating have higher coating thickness and surface roughness values compared with less number of layers coating from same type of layer's materials.

  • •

    Samples with high number of layers coating have higher hardness value compared with less number of layers coating from same type of layer's materials.

  • •

    Negative bacteria showed resistance to all substances, while positive bacteria showed resistance to all substances except samples coated with one and two-layer HA-ZnO coating.

  • •

    The electrochemical studies confirm that layer coatings have superior anti-corrosion properties.

Therefore, coated DSS alloy by vacuum spin coating device can be considered a promising biomaterial for tissue replacement.

Authors contributions

Nesreen Dakhel Fahad has conducted (1, 2, 3, 4); Nabaa Sattar Radhi has conducted (1, 3, 5); Zainab S.Al-Khafaji has conducted (3, 5) and Abass Ali Diwan has conducted (1, 2, 4).

Acknowledgments

The authors thank university of Kufa and university of Babylon, Iraq. Moreover, this work was supported by Al-Mustaqbal University College (grant number MUC-E-0122).

Contributor Information

Nesreen Dakhel Fahad, Email: nasreend.aboghnim@uokufa.edu.iq.

Nabaa Sattar Radhi, Email: mat.nabaa.sattar@uobabylon.edu.iq.

Zainab S. Al-Khafaji, Email: zainabal-khafaji@uomus.edu.iq.

Abass Ali Diwan, Email: abbas.albosalih@uokufa.edu.iq.

References

  • 1.Pertici G. Introduction to bioresorbable polymers for biomedical. Biores. Polym. Biomed. Appl. From Funda. Transla. Med. 2016;24(1) [Google Scholar]
  • 2.Ratner B.D., et al. In: Sakiyama-Elbert S., Zhang G., Yaszemski M., editors. 3–19. 2013. (Introduction—biomaterials Science: an Evolving, Multidisciplinary Endeavor,” Biomater. Sci. An Introd. To Mater. Med. Wagner). W. [Google Scholar]
  • 3.Radhi N.S., Al-Khafaji Z.S. 2018. Preparation and Investigation Composite Coating (Ni-Nano Hydroxyapatite) on Low Carbon Steel Samples. [Google Scholar]
  • 4.Thomas S., Grohens Y., Ninan N. William Andrew; 2015. Nanotechnology Applications for Tissue Engineering. [Google Scholar]
  • 5.Hamza S., Radhi N.S., Sahi N.M. Study the antibacterial activity of hydroxyapatite-nano silver coating on titanium substrate. J. Phys. Conf. 2021;1973(1) [Google Scholar]
  • 6.Chen Q., Thouas G.A. Metallic implant biomaterials. Mater. Sci. Eng. R Rep. 2015;87:1–57. [Google Scholar]
  • 7.David F. Elsevier; London: 1986. Definitions in Biomaterials: Proceedings of a Consensus Conference of the European Society for Biomaterials. [Google Scholar]
  • 8.Radhi N.S., Hamza S., Ahmed R.T., Sahi N.M. Functionally graded coating (silver/yttria) multi layers by pulsed laser deposition technique on 316L stainless steel substrate. J. Phys. Conf. 2021;1973(1) [Google Scholar]
  • 9.Eliaz N., Hakshur K. Degradation of Implant Materials. Springer; 2012. Fundamentals of tribology and the use of ferrography and bio-ferrography for monitoring the degradation of natural and artificial joints; pp. 253–302. [Google Scholar]
  • 10.Manivasagam G., Dhinasekaran D., Rajamanickam A. Biomedical implants: corrosion and its prevention-a review. Recent patents Corros. Sci. 2010;2(1) [Google Scholar]
  • 11.Burakowski T., Wierzchon T. CRC press; 1998. Surface Engineering of Metals: Principles, Equipment, Technologies. [Google Scholar]
  • 12.Hu C., Ashok D., Nisbet D.R., Gautam V. Bioinspired surface modification of orthopedic implants for bone tissue engineering. Biomaterials. 2019;219 doi: 10.1016/j.biomaterials.2019.119366. [DOI] [PubMed] [Google Scholar]
  • 13.Pawlowski L. Suspension and solution thermal spray coatings. Surf. Coating. Technol. 2009;203(19):2807–2829. [Google Scholar]
  • 14.Kuroda S., Kawakita J., Watanabe M., Katanoda H. Warm spraying—a novel coating process based on high-velocity impact of solid particles. Sci. Technol. Adv. Mater. 9 (3) 2008 doi: 10.1088/1468-6996/9/3/033002. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 15.Fournier E., Devaney R., Palmer M., Kramer J., El Khaja R., Fonte M. Superelastic orthopedic implant coatings. J. Mater. Eng. Perform. 2014;23(7):2464–2470. [Google Scholar]
  • 16.Szatkowski T., et al. Synthesis and characterization of hydroxyapatite/chitosan composites. Physicochem. Probl. Miner. Process. 2015;51 [Google Scholar]
  • 17.Santander S.A., Ossa C.M.L. Stainless steel: material facts for the orthodontic practitioner. Rev. Nac. Odontol. 2015;11 20. [Google Scholar]
  • 18.Association I.M. Vol. 10. IMOA; London, UK: 2009. (Practical Guidelines for the Fabrication of Duplex Stainless Steels). [Google Scholar]
  • 19.Kocijan A., Merl D.K., Jenko M. The corrosion behaviour of austenitic and duplex stainless steels in artificial saliva with the addition of fluoride. Corrosion Sci. 2011;53(2):776–783. [Google Scholar]
  • 20.Gregorutti R.W., Grau J.E., Sives F., Elsner C.I. Mechanical, electrochemical and magnetic behaviour of duplex stainless steel for biomedical applications. Mater. Sci. Technol. 2015;31(15):1818–1824. [Google Scholar]
  • 21.Krolczyk G.M., Maruda R.W., Nieslony P., Wieczorowski M. Surface morphology analysis of duplex stainless steel (DSS) in clean production using the power spectral density. Measurement. 2016;94:464–470. [Google Scholar]
  • 22.Krolczyk G., Nieslony P., Legutko S. Microhardness and surface integrity in turning process of duplex stainless steel (DSS) for different cutting conditions. J. Mater. Eng. Perform. 2014;23(3):859–866. [Google Scholar]
  • 23.Ralls A.M., et al. Tribological and corrosion behavior of high pressure cold sprayed duplex 316 L stainless steel. Tribol. Int. 2022;169 [Google Scholar]
  • 24.Kazasidis M., et al. Microstructure and cavitation erosion performance of nickel-Inconel 718 composite coatings produced with cold spray. Surf. Coating. Technol. 2020;382 [Google Scholar]
  • 25.De Falco G., et al. Antimicrobial activity of flame-synthesized nano-TiO 2 coatings. Environ. Sci. Nano. 2017;4(5):1095–1107. [Google Scholar]
  • 26.De Falco G., et al. TiO2 nanoparticle coatings with advanced antibacterial and hydrophilic properties prepared by flame aerosol synthesis and thermophoretic deposition. Surf. Coating. Technol. 2018;349:830–837. [Google Scholar]
  • 27.Jalvo B., Faraldos M., Bahamonde A., Rosal R. Antimicrobial and antibiofilm efficacy of self-cleaning surfaces functionalized by TiO2 photocatalytic nanoparticles against Staphylococcus aureus and Pseudomonas putida. J. Hazard Mater. 2017;340:160–170. doi: 10.1016/j.jhazmat.2017.07.005. [DOI] [PubMed] [Google Scholar]
  • 28.Schilling K., et al. Human safety review of ‘nano’ titanium dioxide and zinc oxide. Photochem. Photobiol. Sci. 2010;9(4):495–509. doi: 10.1039/b9pp00180h. [DOI] [PubMed] [Google Scholar]
  • 29.Nohynek G.J., Dufour E.K., Roberts M.S. Nanotechnology, cosmetics and the skin: is there a health risk? Skin Pharmacol. Physiol. 2008;21(3):136–149. doi: 10.1159/000131078. [DOI] [PubMed] [Google Scholar]
  • 30.Nohynek G.J., Antignac E., Re T., Toutain H. Safety assessment of personal care products/cosmetics and their ingredients. Toxicol. Appl. Pharmacol. 2010;243(2):239–259. doi: 10.1016/j.taap.2009.12.001. [DOI] [PubMed] [Google Scholar]
  • 31.Cho W.-S., et al. Differential pro-inflammatory effects of metal oxide nanoparticles and their soluble ions in vitro and in vivo; zinc and copper nanoparticles, but not their ions, recruit eosinophils to the lungs. Nanotoxicology. 2012;6(1):22–35. doi: 10.3109/17435390.2011.552810. [DOI] [PubMed] [Google Scholar]
  • 32.Heng B.C., et al. Evaluation of the cytotoxic and inflammatory potential of differentially shaped zinc oxide nanoparticles. Arch. Toxicol. 2011;85(12):1517–1528. doi: 10.1007/s00204-011-0722-1. [DOI] [PubMed] [Google Scholar]
  • 33.Boraschi D., Costantino L., Italiani P. Interaction of nanoparticles with immunocompetent cells: nanosafety considerations. Nanomedicine. 2012;7(1):121–131. doi: 10.2217/nnm.11.169. [DOI] [PubMed] [Google Scholar]
  • 34.Boscolo P., et al. Effects of palladium nanoparticles on the cytokine release from peripheral blood mononuclear cells of non-atopic women. J. Biol. Regul. Homeost. Agents. 2010;24(2):207–214. [PubMed] [Google Scholar]
  • 35.Greulich C., et al. Cell type-specific responses of peripheral blood mononuclear cells to silver nanoparticles. Acta Biomater. 2011;7(9):3505–3514. doi: 10.1016/j.actbio.2011.05.030. [DOI] [PubMed] [Google Scholar]
  • 36.Vallhov H., et al. Adjuvant properties of mesoporous silica particles tune the development of effector T cells. Small. 2012;8(13):2116–2124. doi: 10.1002/smll.201102620. [DOI] [PubMed] [Google Scholar]
  • 37.Sabzi M., Far S.M., Dezfuli S.M. Characterization of bioactivity behavior and corrosion responses of hydroxyapatite-ZnO nanostructured coating deposited on NiTi shape memory alloy. Ceram. Int. 2018;44(17):21395–21405. [Google Scholar]
  • 38.Dezfuli S.M., Sabzi M. Deposition of ceramic nanocomposite coatings by electroplating process: a review of layer-deposition mechanisms and effective parameters on the formation of the coating. Ceram. Int. 2019;45(17):21835–21842. [Google Scholar]
  • 39.Mersagh Dezfuli S., Sabzi M. A study on the effect of presence of CeO2 and benzotriazole on activation of self‐healing mechanism in ZrO2 ceramic‐based coating. Int. J. Appl. Ceram. Technol. 2018;15(5):1248–1260. [Google Scholar]
  • 40.Geuli O., Lewinstein I., Mandler D. Composition-tailoring of ZnO-hydroxyapatite nanocomposite as bioactive and antibacterial coating. ACS Appl. Nano Mater. 2019;2(5):2946–2957. [Google Scholar]
  • 41.Joost U., et al. Photocatalytic antibacterial activity of nano-TiO2 (anatase)-based thin films: effects on Escherichia coli cells and fatty acids. J. Photochem. Photobiol. B Biol. 2015;142:178–185. doi: 10.1016/j.jphotobiol.2014.12.010. [DOI] [PubMed] [Google Scholar]
  • 42.Mersagh Dezfuli S., Sabzi M. Deposition of self-healing thin films by the sol–gel method: a review of layer-deposition mechanisms and activation of self-healing mechanisms. Appl. Phys. A. 2019;125(8):1–8. [Google Scholar]
  • 43.Dawood N.M., Radhi N.S., Al-khafaji Z.S. Invest. Corros. Wear Behav. Nickel-Nano Silicon Carbide Stainless Steel 316L. 2020;1002:33–43. [Google Scholar]
  • 44.Yeom H., Dabney T., Pocquette N., Ross K., Pfefferkorn F.E., Sridharan K. Cold spray deposition of 304L stainless steel to mitigate chloride-induced stress corrosion cracking in canisters for used nuclear fuel storage. J. Nucl. Mater. 2020;538 [Google Scholar]
  • 45.Burnat B., et al. Surface characterization, corrosion properties and bioactivity of Ca-Doped TiO2 coatings for biomedical applications. Surf. Coating. Technol. 2015;280:291–300. [Google Scholar]
  • 46.Al-Murshdy J.M.S., Hammood A.S., Fahad N.D. Improvement corrosion behaviour of lean duplex stainless steel 2101 alloy in ringer solution by plasma nitriding for biomedical applications. J. Phys. Conf. Ser. 1973;1:2021. doi: 10.1088/1742-6596/1973/1/012070. [DOI] [Google Scholar]
  • 47.Popescu M.C., et al. Antibacterial efficiency of cellulose-based fibers covered with ZnO and Al2O3 by atomic layer deposition. Appl. Surf. Sci. 2019;481:1287–1298. [Google Scholar]
  • 48.He X., et al. Biocompatibility, corrosion resistance and antibacterial activity of TiO2/CuO coating on titanium. Ceram. Int. 2017;43(18):16185–16195. [Google Scholar]
  • 49.Hammood A.S., Mahdi M.A.S., Thair L., Haddad H. Evaluating the effect of hydroxyapatite-chitosan coating on the corrosion behavior of 2205 duplex stainless steel for biomedical applications. Mater. Res. Express. 2019;6(8) [Google Scholar]

Articles from Heliyon are provided here courtesy of Elsevier

RESOURCES