Skip to main content
ACS AuthorChoice logoLink to ACS AuthorChoice
. 2023 Oct 25;15(44):51558–51564. doi: 10.1021/acsami.3c10564

2D High-Temperature Superconductor Integration in Contact Printed Circuit Boards

Christian N Saggau †,*, Sanaz Shokri †,‡, Mickey Martini †,‡, Tommaso Confalone †,‡, Yejin Lee †,‡, Daniel Wolf †, Genda Gu §, Valentina Brosco ⬡,⬢, Domenico Montemurro ⊥, Valerii M Vinokur #,∇, Kornelius Nielsch †,‡,○, Nicola Poccia †,*
PMCID: PMC10637321  PMID: 37878903

Abstract

graphic file with name am3c10564_0005.jpg

Inherent properties of superconducting Bi2Sr2CaCu2O8+x films, such as the high superconducting transition temperature Tc, efficient Josephson coupling between neighboring CuO layers, and fast quasiparticle relaxation dynamics, make them a promising platform for advances in quantum computing and communication technologies. However, preserving two-dimensional superconductivity during device fabrication is an outstanding experimental challenge because of the fast degradation of the superconducting properties of two-dimensional flakes when they are exposed to moisture, organic solvents, and heat. Herein, to realize superconducting devices utilizing two-dimensional (2D) superconducting films, we develop a novel fabrication technique relying on the cryogenic dry transfer of printable circuits embedded into a silicon nitride membrane. This approach separates the circuit fabrication stage requiring chemically reactive substances and ionizing physical processes from the creation of the thin superconducting structures. Apart from providing electrical contacts in a single transfer step, the membrane encapsulates the surface of the crystal, shielding it from the environment. The fabricated atomically thin Bi2Sr2CaCu2O8+x-based devices show a high superconducting transition temperature of Tc ≃ 91 K close to that of the bulk crystal and demonstrate stable superconducting properties.

Keywords: 2D materials, contact printing, via contacts, high-temperature superconductivity

Introduction

The Bi2Sr2CaCu2O8+x (BSCCO) cuprate having the d-wave pairing symmetry1 and displaying superconductivity even when being a monolayer2,3 is an ideal candidate for building highly functional quantum devices. Twisted van der Waals (vdW) heterostructures composed of BSCCO layers were predicted4−6 to break time-reversal symmetry at certain twist angles, a phenomenon that was demonstrated experimentally.7 As such, BSCCO twisted heterostructures could potentially lead to topological states and Majorana modes.8 Additionally, twisted interfaces between cuprate crystals have been proposed as an adaptable platform for Josephson junctions with controllable coupling,9−14 which is a desirable feature for quantum applications. Thin BSCCO films promise to become an important platform for quantum sensors and detectors since bolometers fabricated from thin structured BSCCO crystals demonstrated a high level of single-photon sensitivity above 25 K.15,16 Yet, the main challenge for building these structures is to maintain the superconducting phase of thin BSCCO crystals while integrating them into an electrical circuit, as the oxygen dopants are mobile at temperatures exceeding 200 K.17,18 Furthermore, thin BSCCO flakes easily react with water leading to structural changes and modification of the oxygen doping level, which is crucial since altering the doping can drive the BSCCO film into an insulating phase.19−22 The preservation of interface superconductivity of the BSCCO crystal has been recently achieved by means of a cryogenic exfoliation technique combined with a solution-free stencil mask approach, enabling the fabrication of electrical devices entirely in an inert atmosphere.13,14,23 The bottleneck hindering the realization of functional integrated circuits based on cuprate superconductors is the metallization of atomically thin crystals. The previously mentioned stencil mask approach enables the realization of simple electrical contacts in a single-layer geometry through the thermal evaporation of relatively low melting metals, such as gold, while providing a resolution down to 1 μm.3 However, highly energetic metal clusters and atoms bombarding the surface of the crystal during the deposition alter its doping level near the contact region due to local heating. To circumvent crystal distortions associated with the metallization process, different cold lamination techniques were developed for other vdW materials. These include the direct transfer of metal films,24 contacts attached to the bottom of poly(methyl methacrylate) (PMMA) sheets,25,26 metal deposition by inkjet printing,27 and contacts integrated into the h-BN flakes.28,29 However, all these methods have certain limitations making them unsuitable for integrating complex circuits with materials as sensitive as BSCCO. The first two approaches are limited to simple contact geometries with a minimal feature size of around 3 μm.24−26 Similarly, printed contacts have a comparably low resolution in the range of tens of microns and require an annealing step to obtain an acceptable electrical conductivity.30 The BSCCO itself can be damaged during annealing or printing due to heating or chemical reactions with the binders and solvents of the ink. In contrast, via contacts embedded within h-BN flakes can provide a submicron resolution and avoid direct lithographic patterning onto the 2D crystal.28,29 Nevertheless, the h-BN flakes cannot host complex circuits as a consequence of their small size, additional time-consuming processes, such as lithography and metalisation are required to obtain a functional device.28,29 To overcome these limitations, we develop a novel via contact method that relies on the dry cryogenic placement with a poly(dimethylsiloxane) (PDMS) stamp31 to transfer electrical circuits embedded within inorganic SiNx nanomembranes. We employ this experimental technique to fabricate and measure a Hall bar device based on an atomically thin BSCCO crystal. We show that this technology offers a unique opportunity to introduce cuprate heterostructures in complex circuits, such as microwave resonant superconducting circuits, widely used in the field of optoelectronics32,33 and quantum computing.34

Experimental Section

Contact Printed Microcircuit Boards

The SiNx membrane acts as a transferable microcircuit board (μCB) hosting all of the necessary electrical circuitry. The contact formation is completely decoupled from the realization of the electrical contact lines and dielectric barriers that are produced by traditional complementary metal-oxide-semiconductor (CMOS) processes. A 2D thin crystal is electrically contacted by bottom contacts, which are connected through via contacts with the contacting pads and contact lines at the top surface of the membrane. Upon contact printing of the membrane, as illustrated in Figure 1, the device can be directly wire-bonded to a standard chip carrier enabling its electrical characterization. In addition to providing electrical contacts, the membrane acts as a barrier to the environment, facilitating the handling of the integrated 2D material.

Figure 1.

Figure 1

Schematic illustration of the general process flow. (1) Microelectronic circuit boards are fabricated with classical CMOS processes in a highly parallel fashion. (2) Embedded via contacts enable hybrid devices through contact printing of the circuits onto a 2D material. (3) Direct wire bonding facilitates fast and easy characterization.

The fabrication of the membranes starts with a silicon-on-insulator (SOI) substrate (Figure 2a I), where the silicon device layer acts as a sacrificial layer later on, enabling the creation of a freestanding transferable circuit. A 5 nm thick Al2O3 layer is deposited by atomic layer deposition (50 cycles ALD) onto the cleaned surface of the substrate. The bottom metal contacts are created, in the following step, on top of the Al2O3 layer, by ultraviolet (UV) or electron beam lithography (EBL), sputter deposition, and lift-off (Figure 2a II). The whole sample is subsequently covered by a 500 nm thick SiNx layer deposited by plasma-enhanced chemical vapor deposition (PECVD). A similar dielectric stack was used previously as a strain engineering platform to form three-dimensional devices, such as capacitors and optical resonators.35,36 After the deposition of the SiNx layer, the via contacts connecting the bottom and the top surfaces of the membrane are formed. They are fabricated by a two-step process. First, holes are etched by reactive ion etching (RIE) reaching the bottom metal layers (Figure 2a III). Then, the via and electrical conduction lines are created on the top surface by using lithography and lift-off (Figure 2a IV). In the following step, the SiNx film is structured to form quadratic individually releasable membranes with a side length of 550 μm hosting tethers at each corner. The tethers are needed to keep the membranes in place once they are released. Additionally, they enable the picked up with a polymer stamp (Figure 2a V). The individual membranes are then isolated from each other through the creation of 5 μm wide trenches, reaching the buried oxide (BOX) layer. These trenches are formed in the bare silicon by deep reactive ion etching (DRIE). The whole sample is afterward passivated with a 5 nm thin Al2O3 layer (50 cycles ALD). The coated trenches suppress the side-ward propagation of the etch front, limiting the release to a restricted area below the μCBs. In the following step, access windows are created in the Al2O3 layer (RIE: BCl3, Cl2, Ar), enabling XeF2 gas to access the Si sacrificial layer (Figure 2a VII). After the release is finished, the whole chip is immersed for 5 min in a tetramethylammonium hydroxide (TMAH) solution to dissolve the Al2O3 passivation. After that, the chip is transferred to isopropanol and critical point dried (CPD), see Figure 2a VIII. After CPD, the chip hosting the μCB is ready to use. More details on the fabrication can be found in the Supporting Information (Figure S2). A freestanding, transferable circuit hosting a Hall bar structure is shown in Figure 2b. The central bottom side area of a membrane is displayed in Figure 2b 1, while it is attached to a PDMS stamp. The bottom contacts, which recline on the surface of the 2D material under investigation, are clearly visible. For the EBL-exposed structures, 500 nm wide contact lines with the sub 200 nm resolution are obtained, demonstrating a clear advantage in comparison with previous approaches for contact printed contacts (see Figure 2b 1–3). Figure 2c displays a representative bonded device based on a thin BSCCO crystal. To reveal the sharpness of the interface between the crystal and the electrical contact at atomic resolution, we perform cross-sectional high-annular dark-field scanning transmission electron microscopy (HAADF-STEM) in the region indicated in Figure 3a. The TEM image is shown in Figure 3b,c with different magnifications. The gold layer reclines perfectly on the thin crystal, displaying a flat edge. Bright spots correspond to the heavy Bi atoms that terminate in each layer of the BSCCO crystal. At the top and bottom surfaces of the BSCCO crystal, a subunit cell degraded region (dark area) can be observed due to a 30 min exposure of the flake to the glovebox atmosphere (Ar: 99.999%, O2 ≤ 0.1 ppm, H2O ≤ 0.1 ppm) between the crystal exfoliation and the stacking of the membrane on top of it. In our system, we are able to preserve interface superconductivity and crystalline order in regions exposed less than 1 min to the Ar atmosphere at cryogenic temperatures.13,14 A pristine BSCCO/Au interface can thus be created by a quick stacking of the circuit on top of the crystal, which is, however, beyond the scope of the present study.

Figure 2.

Figure 2

(a) Schematic illustration of the fabrication process. (I) The SOI substrate; (II) the Al2O3 passivated substrate with Au bottom contacts; (III) the SiNx deposition and via etching; (IV) the contact pad definition and via filling; (V) the definition of the membrane by RIE and (VI) DRIE; (VII) the passivation of the top surface and opening of access windows; (VIII) the release of the membrane and the isotropic removal of the passivation layer. (b) Microscopic image of a released microcircuit board. Subpanels (1–3) show the bottom side of membranes. The bottom contacts can be distinguished by their difference in color. Subpanel (1) shows optical lithographically patterned structures, while subpanel (2) shows a scanning electron microscope (SEM) image of the EBL-written one. Subpanel (3) shows the magnification of the bottom contacts shown in (b) (2). (c) The microscopy image of a bonded Hall bar device.

Figure 3.

Figure 3

(a) Sketch of a cut through the central part of the membrane illustrating the via and bottom contacts. The red dashed rectangle indicates the region investigated by cross-sectional high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM). (b) The HAADF-STEM image of a BSCCO/Au interface. (c) Zoom into the region within the dashed green rectangle in (b). The Bi atoms are most notably resolved as bright spots due to their high atomic mass.

Results and Discussion

Superconducting Hall Devices

To demonstrate the strength of this novel via contact technique, a BSCCO Hall device is fabricated from an atomically thin crystal. The schematic illustration of the fabrication process, along with experimental details, is reported in Figure S2 in the Supporting Information (SI). In the first place, the chip hosting the μCBs is placed on a liquid nitrogen-cooled stage kept at −30 °C. A PDMS stamp is then brought into contact with a μCB, utilizing a micromanipulator, and let it thermalize to enhance its stickiness. By quickly detaching the stamp from the chip, we pick up the target membrane hosting the circuit. Next, the BSCCO flakes are exfoliated at room temperature via the Scotch tape method on a SiO2/Si substrate, previously treated with oxygen plasma to enhance the vdW forces between BSCCO and SiO2, and baked overnight (180 °C) to desorb water molecules. By optical contrast, we identify a very thin flake (≃13.5 nm), as shown in Figure 4a, and align the membrane before the contact printing. Finally, the sample is slowly heated to room temperature, followed by the slow removal of the PDMS stamp. One of the key advantages of our technique is that the electrical contacts are established at low temperatures within a few minutes after the crystals cleave before the top layers of the cuprate crystal strongly degrade. Figure 4b displays a close-up of the contact area of the device right after printing the μCB onto the BSCCO flake. Our protocol allows for extremely clean electrical contacts to BSCCO with an areal resistance <35 kΩ μm–2. The observed contact resistances are similar to the one obtained by evaporation, while for transfer-printed contacts, a lower parameter spread is observed (Figure S5). Additionally, evaporated, low ohmic contacts sometimes show indications of degradation, which we do not observe for transfer-printed ones. For example, some samples with evaporated contacts show a reminiscent low resistance below Tc and an increase of the resistance upon reaching a resistance below the noise floor if the temperature is further decreased. Occasionally, no superconducting transition is observed at all. The high electronic quality of our fabricated device is also revealed in Figure 4c, which reports the four-point sheet resistance for the Hall device measured right after its fabrication (I) and after storing the sample for 10 days in an Ar-filled glovebox at −40 °C (II). The two data sets show nearly identical inflection points of 91.45 and 91.50 K, respectively. The small changes in the Tc and the sheet resistance can be explained by the loss of oxygen dopants, as even storage at −40 °C cannot totally prevent a degradation of the sample over time. To totally stop the loss of dopants, even lower temperatures are required, as the mobile oxygen is frozen out at temperatures below 200 K.17,18 To arrive at a consistent theoretical description, the behavior of the system across the metal–insulator transition (SIT) is analyzed employing the theory of two-dimensional superconducting fluctuations.3,37 The scattering time τ is taken as approximately 0.1 ps, while the inelastic scattering time τφ and the critical temperature Tc are extracted from the fits. For the two sets of data (see Table 1), we get similar results, with slightly larger Tc and τφ observed for the data shown in Figure 4c I, the sample being measured immediately after its fabrication. In both cases, the critical temperature estimated from the fits is close to the inflection point of the experimental data, and it is identical to the value reported for the optimally doped bulk crystal,38 demonstrating a device with pristine and stable superconducting properties. This is confirmed by monitoring the values of the contact resistance and the critical superconducting temperature for a 40 nm thick crystal over several weeks (Figure 4d). All these findings suggest that our methodology based on the transfer of μCB preserves the superconducting properties of the BSCCO crystal and that the membrane acts as an encapsulation layer, blocking the detrimental effects of disorder over a long time. The robustness of the membrane is demonstrated by the numerous thermal cycles performed for our experiments. The Hall resistance and the magnetoresistance of the thin device (shown in Figure 4a) and the corresponding theoretical analysis are presented in the SI.

Figure 4.

Figure 4

(a) Microscopy image of the BSCCO crystal with a thickness of ≃13.5 nm (4.5 unit cells). (b) Close-up of the device consisting of the flake contacted by a μCB. (c) Sheet resistance (left axis) of the crystal across the superconducting transition measured right after the fabrication of the device (I) and after 10 days (II). The black solid and green dashed lines correspond to the experimental data and the fit, respectively. The red curves (right axis) represent the derivative of the experimental data displaying the inflection point Tinf. The fitting parameters are τφ = 0.38 ns, τ = 0.1 ps, and Tc = 91.28 K for case (I); τφ = 0.36 ns, τ = 0.1 ps, and Tc = 91.39 K for case (II). (d) Mean areal contact resistance at room temperature (left axis) and the inflection point Tinf (right axis) of a 40 nm thick BSCCO flake measured over time. Between each measurement, the sample is stored in an Ar atmosphere and kept at −40 °C between #1 and #5 and at room temperature between #5 and #6.

Table 1. Fitting Parameters for Superconducting Transition.

set Tc τφ τ
Figure 4 (I) 91.28 K 0.38 ns 0.1 ps
Figure 4 (II) 91.39 K 0.36 ns 0.1 ps

Conclusions

In summary, we demonstrate a novel route to integrate sensitive and thin BSCCO crystals into complex nanodevices. This integration is achieved by the cryogenic dry transfer of microcircuits embedded in an inorganic dielectric nanomembrane, where the via contacts connect the bottom electrical contacts to the 2D crystal with contact lines formed on the top surface of the membrane. Additionally, the membrane provides a physical barrier to the environment, which enables the handling of sensitive devices in ambient conditions. Employing this fabrication technique, we realize an atomically thin BSCCO device with high-quality electrical contacts (areal resistance <35 kΩ μm–2), exhibiting pristine and stable superconducting properties for a very long time (TC ≃ 91.5 K). Our technology, with the capability to realize high-resolution contact lines on multiple levels and through the use of inorganic dielectrics, provides an effective path toward the implementation of electric gates necessary for individually tunable devices, a core requirement for complex integrated circuits.

Methods

Microcircuit Boards

The SOI wafers are purchased from Ultrasil and diced into 10 mm × 10 mm substrates before use. The substrates are cleaned for 10 min under mild ultrasonication in a bath of (1) hot dimethyl sulfoxide (DMSO) (120 °C), (2) acetone, and (3) isopropanol. The samples are then blow-dried under nitrogen flow and cleaned in an O2 plasma for 30 min (Diener Pico). Below, we provide the details of each process section of fabrication.

ALD

Al2O3 is deposited by the ALD Arradiance GEMstar at 280 °C with H2O and trimethylaluminum as precursors.

PECVD

SiNx is deposited by PECVD (Sentech Si500D) at 280 °C with SiH4 (5% in He) (50 sccm) and N2 (80 sccm) as precursors. The pressure is p = 0.019 mbar, and the power of the inductively coupled plasma (ICP) is P = 200 W.

RIE

SiNx is etched using Oxford instruments - Plasmalab 80 system. Bias voltage U = 155 V, ICP-Power P = 50 W, and T = 30 °C, and the precursors are CF4 with a flow of 10 sccm, CHF3 at 20 sccm, and O2 at 4 sccm.

RIE

Al2O3 is etched under the same conditions but with different precursors (BCl3 at 20 sccm, Cl2).

RIE

Si is etched using SF6 at 80 sccm and O2 at 8 sccm as precursors (ICP-Power P = 450 W, bias voltage U = −30 V, and T = 120 °C).

Lithography

Resist AZ5214E is spun onto samples at 4500 rpm and prebaked for 180 s on a hot plate at 90 °C. The samples are then exposed to a maskless aligner (Heidelberg MLA 100). For all etching steps, the resist is used as a positive (dose of 90 mJ cm–1). The samples are finally developed for 60 s with AZ 726 MIF. For the lift-off, a negative slope is used (dose = 30 mJ cm–2, postbaking for 450 s at 120 °C, and flood exposure for 45 s). For the definition of the bottom contacts, the development process lasts 45 s (with AR 300–35), while for top contacts it lasts 16 s (with AZ 726 MIF).

Metallization

Contacts are sputtered using the Torr CRC600 Series tool. Gold bottom contacts are deposited with a rate of Ås–1 for a total thickness of 80 nm. The top contacts are formed by depositing 5 nm of Cr at a rate of 1 Ås–1 and 80 nm of Au at 1 Ås–1. Lift-off is performed in DMSO overnight.

Release

The samples are exposed in a gas phase etcher (SPTS, Xactix) to multiple cycles (60 s exposure) of XeF2 vapor (4 mbar) until the membranes are completely freestanding. The progress of the release is monitored with an optical microscope. The released membranes are immersed into an alkali developer (AZ 726 MIF) for 5 min to remove the bottom Al2O3 layer, transferred for 10 min into H2O, before being transferred into isopropanol overnight. The prepared sample is then CPD dried and baked overnight on a hot plate at 125 °C to remove residual water.

Cleaving of BSCCO

Floating-zone grown Bi2Sr2CaCu2O8+d crystals cut orthogonal to the c-axis are mechanically exfoliated inside a high purity argon-filled glovebox (MBraun H2O < 0.1 ppm, O2 < 0.1 ppm), onto Si/SiO2 substrates via the Scotch tape method (3 M, Scotch magic tape). Rectangular flakes with a desired size (L ≥ 100 μm, w ≥ 40 μm, and thickness h ≤ 40 nm) are selected under an optical microscope.

Electrical Characterization

After transferring a μCB onto a BSCCO thin flake, the sample is glued onto a sample holder with silver glue and bonded under ambient conditions (FS Bondtec 58 series). The sample is loaded into a cryostat (Quantum Design PPMS), and the electronic characteristics are recorded with a lock-in amplifier (Stanford Research Systems SR830). The Hall and magnetoresistance data shown in the SI are symmetrized to exclude geometric effects. The electrical characterization of Figure 4d is performed in a cryostat (Quantum Design Versalab). The circuit used to evaluate the contact resistance is shown in Figure S4 and the spread of the contact resistance for contact printed and evaporated contacts is shown in Figure S5. The injected current is I = 5 μA for 1–2 and 4–6. For 3, the injected current is I = 10 μA.

Acknowledgments

The authors thank the Deutsche Forschungsgemeinschaft for financial support (DFG 452128813, DFG 512734967, DFG 492704387, and DFG 460444718). The work of V.M.V. and C.N.S. was supported by Terra Quantum AG and partly by the NSF 2105048 (V.M.V). V.B. acknowledges financial support from: PNRR MUR project PE0000023-NQSTI. The authors are grateful to Heiko Reith and Ronny Engelhard for providing access to cleanroom infrastructure and Nicolas Perez Rodriguez for providing access to cryogenic measurement facilities. The authors thank Henk-Willem Veltkamp for technical support at the MESA+ facility. The authors thank Thomas Wiek for the preparation of the TEM lamella. The work at BNL was supported by the US Department of Energy, Office of Basic Energy Sciences, contract no. DOE-sc0012704. The authors are also grateful to S.Y. Frank Zhao, Philip Kim, Hans Hilgenkamp, and Francesco Tafuri for illuminating and fruitful discussions.

Supporting Information Available

The Supporting Information is available free of charge at https://pubs.acs.org/doi/10.1021/acsami.3c10564.

  • Description of the experimental methodology and fabrication methods; furthermore, a detailed analysis of the Hall data is provided (PDF)

  • 2D high-temperature superconductor integration in contact printed circuit boards (ZIP)

Author Contributions

◆ C.N.S. and S.S. contributed equally to this work. N.P. supervised the experiment; C.N.S. and N.P. conceived the microprinted contacts and their cryogenic transfer methodology; C.N.S., S.S., and Y.L. performed the experiments and analyzed the data with the contribution of V.B., T.C., and V.M.V.; D.W. performed the HAADF-STEM analysis. The theoretical analysis of the Hall effect was done by V.B. and V.M.V. The cuprate crystals were provided by G.G. The fabrication procedure and the results were discussed by C.N.S., S.S., D.M., V.M.V., K.N., and N.P. The manuscript was written by C.N.S., M.M., V.B., V.M.V., K.N., and N.P.; all authors discussed the manuscript.

The authors declare no competing financial interest.

Supplementary Material

am3c10564_si_001.pdf (14.6MB, pdf)
am3c10564_si_002.zip (12.1MB, zip)

References

  1. Tsuei C. C.; Kirtley J. Pairing Symmetry in Cuprate Superconductors. Rev. Mod. Phys. 2000, 72, 969–1016. 10.1103/RevModPhys.72.969. [DOI] [PubMed] [Google Scholar]
  2. Yu Y.; Ma L.; Cai P.; Zhong R.; Ye C.; Shen J.; Gu G. D.; Chen X. H.; Zhang T. High-temperature Superconductivity in Monolayer Bi2Sr2CaCu2O8+δ. Nature 2019, 575, 156–163. 10.1038/s41586-019-1718-x. [DOI] [PubMed] [Google Scholar]
  3. Zhao S. F.; Poccia N.; Panetta M. G.; Yu C.; Johnson J. W.; Yoo H.; Zhong R.; Gu G.; Watanabe K.; Taniguchi T.; Postolova S. V.; Vinokur V. M.; Kim P. Sign-reversing Hall Effect in Atomically Thin High-temperature Bi2.1Sr1.9CaCu2.0O0+δ Superconductors. Phys. Rev. Lett. 2019, 122, 247001 10.1103/PhysRevLett.122.247001. [DOI] [PubMed] [Google Scholar]
  4. Can O.; Tummuru T.; Day R. P.; Elfimov I.; Damascelli A.; Franz M. High-temperature Topological Superconductivity in Twisted Double-layer Copper Oxides. Nat. Phys. 2021, 17, 519–524. 10.1038/s41567-020-01142-7. [DOI] [Google Scholar]
  5. Tummuru T.; Lantagne-Hurtubise S.; Franz E. Twisted Multilayer Nodal Superconductors. Phys. Rev. B 2022, 106, 014520 10.1103/PhysRevB.106.014520. [DOI] [Google Scholar]
  6. Liu Y.-B.; Zhou J.; Yang F.. Making Chiral Topological Superconductivities from Non-topological Superconductivities Through the Twist, 2023. arXiv:2301.07553. arXiv.org e-Print archive. https://arxiv.org/abs/2301.07553 (accessed Aug 29, 2023).
  7. Margalit G.; Yan B.; Franz M.; Oreg Y. Chiral Majorana Modes via Proximity to a Twisted Cuprate Bilayer. Phys. Rev. B 2022, 106, 205424 10.1103/PhysRevB.106.205424. [DOI] [Google Scholar]
  8. Mercado A.; Sahoo S.; Franz M. High-temperature Majorana Zero Modes. Phys. Rev. Lett. 2022, 128, 137002 10.1103/PhysRevLett.128.137002. [DOI] [PubMed] [Google Scholar]
  9. Volkov P. A.; Zhao S. Y. F.; Poccia N.; Cui X.; Kim P.; Pixley J. H.. Josephson Effects in Twisted Nodal Superconductors. 2021, arXiv:2108.13456. arXiv.org e-Print archive. https://arxiv.org/abs/2108.13456 (accessed Aug 29, 2023).
  10. Tummuru T.; Plugge S.; Franz M. Josephson Effects in Twisted Cuprate Bilayers. Phys. Rev. B 2022, 105, 064501 10.1103/PhysRevB.105.064501. [DOI] [Google Scholar]
  11. Volkov P. A.; Wilson J. H.; Lucht K. P.; Pixley J. Current- and Field-induced Topology in Twisted Nodal Superconductors. Phys. Rev. Lett. 2023, 130, 186001 10.1103/PhysRevLett.130.186001. [DOI] [PubMed] [Google Scholar]
  12. Volkov P. A.; Wilson J. H.; Lucht K. P.; Pixley J. Magic Angles and Correlations in Twisted Nodal Superconductors. Phys. Rev. B 2023, 107, 174506 10.1103/PhysRevB.107.174506. [DOI] [PubMed] [Google Scholar]
  13. Lee Y.; Martini M.; Confalone T.; Shokri S.; Saggau C. N.; Wolf D.; Gu G.; Watanabe K.; Taniguchi T.; Montemurro D.; Vinokur V. M.; Nielsch K.; Poccia N. Encapsulating High-temperature Superconducting Twisted van der Waals Heterostructures Blocks Detrimental Effects of Disorder. Adv. Mater. 2023, 35, 2209135 10.1002/adma.202209135. [DOI] [PubMed] [Google Scholar]
  14. Martini M.; Lee Y.; Confalone T.; Shokri S.; Saggau C. N.; Wolf D.; Gu G.; Watanabe K.; Taniguchi T.; Montemurro D.; Vinokur V. M.; Nielsch K.; Poccia N. Twisted Cuprate van der Waals Heterostructures with Controlled Josephson Coupling. Mater. Today 2023, 67, 106–112. 10.1016/j.mattod.2023.06.007. [DOI] [PubMed] [Google Scholar]
  15. Seifert P.; Retamal J. R. D.; Merino R. L.; Sheinfux H. H.; Moore J. N.; Aamir M. A.; Taniguchi T.; Watanabe K.; Kadowaki K.; Artiglia M.; Romagnoli M.; Efetov D. K. A High-Tc van der Waals Superconductor Based Photodetector with Ultra-high Responsivity and Nanosecond Relaxation Time. 2D Mater. 2021, 8, 0350533 10.1088/2053-1583/ac072f. [DOI] [Google Scholar]
  16. Charaev I.; Bandurin D. A.; Bollinger A. T.; Phinney I. Y.; Drozdov I.; Colangelo M.; Butters B. A.; Taniguchi T.; Watanabe K.; He X.; Medeiros O.; Bozovic I.; Božović I.; Jarillo-Herrero P.; Jarillo-Herrero P.; Berggren K. K. Single-photon Detection Using High-temperature Superconductors. Nat. Nanotechnol. 2023, 18, 343–349. 10.1038/s41565-023-01325-2. [DOI] [PubMed] [Google Scholar]
  17. Fratini M.; Poccia N.; Ricci A.; Campi G.; Burghammer M.; Aeppli G.; Bianconi A. Scale-free Structural Organization of Oxygen Interstitials in La2CuO4+y. Nature 2010, 466, 841–844. 10.1038/nature09260. [DOI] [PubMed] [Google Scholar]
  18. Poccia N.; Fratini M.; Ricci A.; Campi G.; Barba L.; Vittorini-Orgeas A.; Bianconi G.; Aeppli G.; Bianconi A. Evolution and Control of Oxygen Order in a Cuprate Superconductor. Nat. Mater. 2011, 10, 733–736. 10.1038/nmat3088. [DOI] [PubMed] [Google Scholar]
  19. Novoselov K. S.; Jiang D.; Schedin F.; Booth T. J.; Khotkevich V. V.; Morozov S. V.; Geim A. K. Two-dimensional Atomic Crystals. Proc. Natl. Acad. Sci. U.S.A. 2005, 102, 10451–10453. 10.1073/pnas.0502848102. [DOI] [PMC free article] [PubMed] [Google Scholar]
  20. Song D.; Zhang X.; Lian C.; et al. Visualization of Dopant Oxygen Atoms in a Bi2Sr2CaCu2O8+δ Superconductor. Adv. Funct. Mater. 2019, 29, 1903843 10.1002/adfm.201903843. [DOI] [Google Scholar]
  21. Sandilands L. J.; Reijnders A. A.; Su A. H.; Baydina V.; Xu Z.; Yang A.; Gu G.; Pedersen T.; Borondics F.; Burch K. S. Origin of the Insulating State in Exfoliated High-Tc Two-dimensional Atomic Crystals. Phys. Rev. B 2014, 90, 081402 10.1103/PhysRevB.90.081402. [DOI] [Google Scholar]
  22. Huang Y.; Zhang L.; Zhou X.; et al. Unveiling the Degradation Mechanism of High-Temperature Superconductor Bi2Sr2CaCu2O8+δ in Water-bearing Environments. ACS Appl. Mater. Interfaces 2022, 14, 39489–39496. 10.1021/acsami.2c08997. [DOI] [PubMed] [Google Scholar]
  23. Zhao S. Z. F.; Poccia N.; Cui X.; Volkov P. A.; Yoo H.; Engelke R.; Ronen Z.; Zhong R.; Gu S.; Plugge G.; Tummuru T.; Franz M.; Pixley J. H.; Kim P.. Emergent Interfacial Superconductivity Between Twisted Cuprate Superconductors. 2021, arXiv:2108.13455. arXiv.org e-Print archive. https://arxiv.org/abs/2108.13455 (accessed:Aug 29, 2023).
  24. Liu G.; Tian Z.; Yang Z.; Xue Z.; Zhang M.; Hu X.; Wang Y.; Yang Y.; Chu P. K.; Mei Y.; Liao L.; Hu W.; Di Z. Graphene-assisted Metal Transfer Printing for Wafer-Scale Integration of Metal Electrodes and Two-dimensional Materials. Nat. Electron. 2022, 5, 275–280. 10.1038/s41928-022-00764-4. [DOI] [Google Scholar]
  25. Liu Y.; Guo J.; Zhu E.; Liao L.; Lee S.-J.; Ding M.; Shakir I.; Gambin V.; Huang Y.; Duan X. Approaching the Schottky–Mott Limit in van der Waals Metal–semiconductor Junctions. Nature 2018, 557, 696–700. 10.1038/s41586-018-0129-8. [DOI] [PubMed] [Google Scholar]
  26. Liu L.; Kong L.; Li Q.; et al. Transferred van der Waals Metal Electrodes for Sub-1-nm MoS2 Vertical Transistors. Nat. Electron. 2021, 4, 342–347. 10.1038/s41928-021-00566-0. [DOI] [Google Scholar]
  27. Zheng W.; Saiz F.; Shen Y.; Zhu K.; Liu Y.; McAleese C.; Conran B.; Wang X.; Lanza M. Defect-free Metal Deposition on 2D Materials via Inkjet Printing Technology. Adv. Mater. 2021, 2104138 10.1002/adma.202104138. [DOI] [PubMed] [Google Scholar]
  28. Telford E. J.; Benyamini A.; Rhodes D.; Wang D.; Jung Y.; Zangiabadi A.; Watanabe K.; Taniguchi T.; Jia S.; Barmak K.; Pasupathy A. N.; Dean C. R.; Hone J. Via Method for Lithography Free Contact and Preservation of 2D Materials. Nano Lett. 2018, 18, 1416–1420. 10.1021/acs.nanolett.7b05161. [DOI] [PubMed] [Google Scholar]
  29. Jung Y.; Choi M. S.; Nipane A.; Borah A.; Kim B.; Zangiabadi A.; Taniguchi T.; Watanabe K.; Yoo W. J.; Hone J.; Teherani J. T. Transferred Via Contacts as a Platform for Ideal Two-dimensional Transistors. Nat. Electron. 2019, 2, 187–194. 10.1038/s41928-019-0245-y. [DOI] [Google Scholar]
  30. Lysień M.; Witczak L.; Wiatrowska A.; Fiaczyk K.; Gadzalinska J.; Schneider L.; Strek W.; Karpinski M.; Kosior L.; Granek F.; Kowalczewski P. Highresolution Deposition of Conductive and Insulating Materials at Micrometer Scale on Complex Substrates. Sci. Rep. 2021, 12, 9327 10.1038/s41598-022-13352-5. [DOI] [PMC free article] [PubMed] [Google Scholar]
  31. Meitl M. A.; Zhu Z.-T.; Kumar V.; Lee K. J.; Feng Y.; Huang Y. Y.; Adesida Il.; Nuzzo R. G.; Rogers J. A. Transfer Printing by Kinetic Control of Adhesion to an Elastomeric Stamp. Nat. Mater. 2006, 5, 33–38. 10.1038/nmat1532. [DOI] [Google Scholar]
  32. Day P. K.; LeDuc H. G.; Mazin B. A.; Vayonakis A.; Zmuidzinas J. A Broadband Superconducting Detector Suitable for Use in Large Arrays. Nature 2003, 425, 817–821. 10.1038/nature02037. [DOI] [PubMed] [Google Scholar]
  33. Natarajan C. M.; Tanner M. G.; Hadfield R. H. Superconducting Nanowire Single-photon Detectors: Physics and Applications. Supercond. Sci. Technol. 2012, 25, 063001 10.1088/0953-2048/25/6/063001. [DOI] [Google Scholar]
  34. Blais A.; Huang R.-S.; Wallraff A.; Girvin S. M.; Schoelkopf R. J. Cavity Quantum Electrodynamics for Superconducting Electrical Circuits: An Architecture for Quantum Computation. Phys. Rev. A 2004, 69, 062320 10.1103/PhysRevA.69.062320. [DOI] [Google Scholar]
  35. Saggau C. N.; Gabler F.; Karnaushenko D. D.; Karnaushenko D.; Ma L.; Schmidt O. G. Wafer-scale High-quality Microtubular Devices Fabricated via Dry-etching for Optical and Microelectronic Applications. Adv. Mater. 2020, 32, 2003252 10.1002/adma.202003252. [DOI] [PubMed] [Google Scholar]
  36. Saggau C. N.; Valligatla S.; Wang X.; Dong H.; Ma L.; Schmidt O. G. Coaxial Micro Ring Arrays Fabricated on Self-assembled Microtube Cavities for Resonant Light Modulation. Laser Photonics Rev. 2022, 16, 2200085 10.1002/lpor.202200085. [DOI] [Google Scholar]
  37. Postolova S. V.; Mironova A. Y.; Baturina T. I. Nonequilibrium Transport Near the Superconducting Transition in TiN Films. JETP Lett. 2014, 100, 635–641. 10.1134/S0021364014220135. [DOI] [Google Scholar]
  38. Wen J. S.; Xu Z. J.; Xu G. Y.; Hücker M.; Tranquada J. M.; Gu G. D. Large Bi-2212 Single Crystal Growth by the Floating-zone Technique. J. Cryst. Growth 2008, 310, 1401–1404. 10.1016/j.jcrysgro.2007.09.028. [DOI] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

am3c10564_si_001.pdf (14.6MB, pdf)
am3c10564_si_002.zip (12.1MB, zip)

Articles from ACS Applied Materials & Interfaces are provided here courtesy of American Chemical Society

RESOURCES