Skip to main content
ACS Omega logoLink to ACS Omega
. 2025 Sep 4;10(38):43391–43403. doi: 10.1021/acsomega.4c08878

Evaluation of a Mining Waste as an Oxygen Carrier for Syngas Production Using Chemical Looping in a 3 kWh Fluidized Bed Reactor

Swagat Das 1, Manas Paliwal 1,*
PMCID: PMC12489697  PMID: 41048749

Abstract

The development of chemical looping (CL) technology depends on oxygen carriers; hence, the purpose of this study is to evaluate the potential of an inexpensive, readily available, and unexplored mining waste for syngas synthesis. In this study, we examined the application of chromite overburden, a byproduct of mining, as an oxygen carrier for the chemical looping reforming of methane. The efficiency of the oxygen carrier was assessed at 750 °C by conducting redox cycles in a fluidized bed reactor, using methane and air as reducing and oxidizing agents, respectively. The reactivity study revealed sustained formation of H2 and CO gases during the reforming process of methane. Phase characterization of the r-oxidized and reduced samples using XRD and SEM unambiguously demonstrated the development of stable phases of chromite and iron oxide, respectively. Phase characterization indicated the formation of a chromite phase after the first oxidation cycle, limiting oxygen transport and slightly reducing the reaction efficiency. The phase analysis showed an overall oxide conversion of 11.11% during the redox cycles. Surface morphologies of unreacted and reacted samples showed no sign of attrition or agglomeration in 20 cycles. Overall, COB achieved a total hydrogen yield of 2736 mL per 10 g OC, with an average H2/CO ratio of 0.87, proving its effectiveness in multicycle chemical looping reforming (CLR). The gas analysis indicated the reduction reactions followed a 3-stage mechanism, i.e., decomposition of methane into carbon and hydrogen, reduction of Fe oxide by H2, CO, and C, and auxiliary reactions involving H2O, CO, CO2, and C. The present work successfully demonstrates the application of chromite overburden (COB) as an oxygen carrier in the production of syngas via a chemical looping reforming scheme.


graphic file with name ao4c08878_0013.jpg


graphic file with name ao4c08878_0011.jpg

1. Introduction

Undoubtedly, human activities are the reason behind global warming, with the global surface temperature rising by 1.1 °C between 2011 and 2020, primarily due to greenhouse gas emissions. Between 2010 and 2019, there has been a continuous rise in greenhouse gas emissions worldwide, with historical and current contributions resulting from unsustainable energy usage. The acceleration of efforts to address climate change at many levels of governance is being driven by international climate accords, growing national objectives for climate action, and growing public awareness. Global energy and carbon intensity have decreased as a result of mitigation measures, with numerous nations attaining GHG emission reductions in the past 10 years. However, the projected worldwide emissions resulting from the measures put into effect by the end of 2020 amount to 57 (52–60) GtCO2-eq in 2030. This indicates a deficiency in implementing the Nationally Determined Contributions (NDCs) of 4 to 7 GtCO2-eq by 2030. If policies are not strengthened, emissions are expected to increase, resulting in a median global warming of 2.2 to 3.5 °C by 2100 (according to the IPCC synthesis report 2023). The objective of limiting anthropogenic global warming to a certain threshold necessitates the restriction of cumulative CO2 emissions, achieving net zero or net negative CO2 emissions and implementing substantial reductions in other greenhouse gas emissions. The achievement of net zero emission objectives depends on the implementation of policies, sustainable energy use, and the development of new technologies.

One of the promising and emerging techniques for clean energy generation is the chemical looping (CL) technique. This technique is an alternative for energy generation through conventional combustion or gasification of carbonaceous fuels. This process consists of two or more reduction and oxidation (redox) steps where carbonaceous fuels are converted to oxidized products by an oxygen carrier particle. Indirect oxygen transfer from oxidants, such as air or steam, to the fuel occurs through the oxygen carrier particles during the redox reaction process. In the reduction step, the role of OC is to donate oxygen to the fuel, resulting in a gaseous mixture of oxidized carbonaceous gases. The oxygen-depleted OC is then replenished in the air reactor in which heat and O2-depleted air is produced. An essential key for the different chemical looping reaction is the type of OCs used in the reaction; its selection and optimization are critical for the novel chemical looping process.

Physicochemical capacity of the OC determines the overall efficiency of the CL processes. Hence, OCs must have desired properties such as better reactivity, thermal stability, good fluidization properties, high mechanical resistance, and resistance to agglomeration and attrition during redox cycles. , Two types of iron-based OCs are currently in focus for CL applications: natural and waste OCs and synthetic OCs. Utilization of synthetic OCs showed greater reactivity and better performance in the process as compared to natural materials. Inherent properties of Fe-based OCs can be enhanced by aiding OCs with inert materials such SiO2, Al2O3, and TiO2. Synthetic OCs are more efficient and show a higher yield of product gases. However, it is noteworthy that the use of ores and industrial residues becomes attractive in industrial applications due to their low costs, abundant availability, and mixed composition; therefore, they can be potential materials for low-cost oxygen carriers in the chemical looping process.

In chemical looping processes, several literature reports have reported the performance of iron ores/waste and ilmenite as an oxygen carrier. For example, Araújo Barros do Nascimento Santiago et al. investigated the performance of Brazilian iron ore, mill scale, and iron spill residue as an oxygen carrier. Their study revealed that Brazilian iron ore (CRJ) exhibited higher O2 transport capacity (R oc = 3.92) and a higher rate index with methane (RICH4 = 13.94%/min and RIair = 12.01%/min). Therefore, this material was chosen for experimentation in the discontinuous fluidized bed reactor. Excellent fuel conversion and reactivity with H2 (H2 > CO > CH4) were shown by CRJ. The conversion also improved with temperature, reaching total combustion in the first reduction period at 950 °C, with X red = 0.113 and X ox = 0.155, suggesting full regeneration. The material exhibited no carbon deposition, minimal attrition loss, and a consistent lifespan of 15,000 h. Furthermore, it retained its reactivity when exposed to hydrogen gas without agglomeration or defluidization problems. Iron ore (81.46% Fe2O3) from the Mentes mine in Turkey was assessed by Dilmaç et al. as an OC for the CLC process under redox cycles in a fluidized bed. They found that the OC remained stable throughout the tests and produced more than 90% of the gaseous products during CL tests using CO fuel gas at 800 °C. Zornoza et al. assessed the redox reactivity of iron-based mineral materials and industrial waste. They specifically focused on promifer industrial waste (100% Fe2O3), which exhibited significant reactivity with CH4, strong mechanical resistance, and favorable fluid dynamic behavior of the particles during redox cycles in a fluidized bed reactor. Condori et al. investigated the CLG of biomass in a 1.5 kWth unit with an iron ore and a manganese ore as an OC for 40 and 48 h, respectively. Their study reported syngas production of around 0.60 N m3/kg of dry biomass for both ores. Furthermore, all the samples achieved excellent biomass conversions (X b > 94%) and carbon conversion efficiencies (ηcc > 95%), demonstrating the process’s potential to prevent CO2 emissions into the environment. While the bed did not exhibit any agglomeration throughout the BCLG process, the attrition rates were significant, resulting in bed life of 160 and 300 h for the manganese and iron ores, respectively. Ilmenite has also been explored as an OC material for CLG of biomass for generating syngas by Condori et al. Their results showed that a product gas consisting of 37–40% CO2, 27–30% H2, 17–21% CO, 10–12% CH4, and 2–3% C2–C3 may be produced under autothermal conditions with a syngas yield of 0.65 N m3/kg dry biomass. In comparison to other gasification processes, the amount of tar generated was comparatively lower, ranging from 1.4 to 3.0 g/kg dry biomass (1 to 2.5 g/Nm3 d.b.). Although ilmenite has a high reduction state in BCLG, it has shown excellent behavior by maintaining high reactivity during operation and avoiding any agglomeration hazards. Nevertheless, the migration of iron (Fe) outward in ilmenite resulted in a 50% reduction in lifespan during the operation of a CLG under appropriate combustion circumstances. Similarly, industrial waste such as red mud has also been explored as an OC material for CLG of biomass to produce syngas. The outcomes of their investigation suggested that increasing the Fe2O3/fuel ratio increases the syngas yield, and after the CLG process, majority of the Fe2O3 in red mud underwent conversion into metallic iron. However, a quantity of wustite and magnetite was seen in the remaining “Straw + Fe2O3” residue, suggesting that red mud had a superior ability to provide oxygen. Crucially, the red mud’s structure remained intact with minimal aggregation during the CLG procedure, allowing for easy regeneration across many successive cycles. Hence, the experimental findings offer a pragmatic and excellent method to gasify crop straw for the generation of syngas while also repurposing red mud from industrial waste as an optimal oxygen carrier.

A further advancement in this research area can be possible by utilizing the abundance and cost-effectiveness of naturally available waste materials within the context of a circular economy, rendering them promising candidates for oxygen carriers in large-scale pilot plant applications. Nickel laterite is a low-grade mineral often found as an overburden in chromite mines. The extraction of chromite ore by opencut mining produces enormous volumes of overburden or chromite overburden (COB). Usually, the overburden (COB) has 0.8–1.5% Ni, 40–50% Fe­(T), and 2–5% Cr2O3. These lean ores possess significant amounts of iron oxide and other transition metal oxides, which means that they might be utilized as an oxygen carrier in the chemical looping reforming of methane to create CO and H2 gases for industrial purposes. In our previous works, we have evaluated the performance of COB as an OC material for methane reforming reaction and 20 redox cycles of CLR using the TGA instrument. The results showed very good stability of the material without any carbon deposition throughout the 20 cycles along with a hydrogen yield of 203.9 mL/g of OC. In order to utilize COB as an OC material in large-scale pilot plant applications, this material needs to be tested in a bigger scale. In this study, we have investigated the performance of COB in a 3 KWh fluidized bed reactor (FBR). The reactivity tests were performed for 20 cycles, with methane as a reducing agent and air as an oxidizing agent. The reacted product reduction and oxidation were analyzed to understand the phase change after reaction. Subsequently, gaseous product distributions and fluidization behavior during redox cycles were examined in a fluidized bed reactor under CL conditions. This will enable the identification of the optimum operating conditions in terms of redox efficiency, fluidization behavior, and lifespan for scaling up in CL processes. This study demonstrates that COB being a mining waste can be a potential low-cost material as an OC material in pilot-scale application of the CL process. This research will be critical in defining the process parameters required for syngas production using naturally available low-grade ores (mining wastes) or industrial wastes as OC materials for the commercial-scale CL process.

2. Materials and Methods

2.1. Materials

This study evaluates the low-cost chromite overburden (COB/laterite ore) as an oxygen carrier. The samples were sourced from the Sukinda region in Odisha, India, and were supplied by Tata Steel Ltd. This sample is an iron oxide-based material. Typically, it possesses a higher iron content (>60%) and includes inert compounds that can serve as chemical supports (SiO2 and Al2O3). The particle size of the as-received sample exhibited a range from fine particles to coarser particles. Consequently, the received particles were categorized into various size ranges through a sieve analysis. Following the sieve analysis, various particle sizes were assessed for their fluidization behavior, revealing that particles within the size range of 150–200 μm exhibited superior fluidization characteristics. Thus, the particles within the size range of 150–200 μm were chosen for the experiments conducted in the fluidized bed reactor.

2.2. Characterization of OC

The samples obtained were subjected to composition analysis using X-ray fluorescence (XRF-Bruker Tiger S8) technology. As stated in our earlier study, the composition analysis of the COB sample showed a greater concentration of iron oxide in addition to inert oxide phases including SiO2 and Al2O3, which may be advantageous for the sample’s redox performance. To further evaluate the morphology of the reacted and unreacted samples, OC characterization was also carried out.

Identification of the phases of the obtained samples and subsequent reduction tests were conducted by using the X-ray diffraction method. The phase identification was performed using an X-ray diffractometer (XRD, Model: D8 Discover, Bruker Corporation). The diffraction patterns were obtained by using the Cu Kα (μ = 0.15418 nm) target over a diffraction angle 2θ, ranging from 10° to 90°, with a step size of 0.02° and a scan speed of 0.2 s/step. Analysis of the XRD findings was conducted using PDF+4 software, which was coupled with the JCPDS crystallographic information database. The unreacted and reacted samples were examined for particle surface morphology and elemental analysis using a field emission scanning electron microscope (ZEISS-MERLIN) coupled with electron-dispersive spectroscopy (EDS). The backscattered mode was utilized to identify the various phases within the particle, while the secondary electron mode was employed to analyze the surface morphology. The Brunauer–Emmett–Teller (BET) analysis was performed to determine the pore size and pore volume of the unreacted and reacted samples. The pore size and pore volume were determined using N2 adsorption–desorption isotherms under liquid nitrogen (at temperature −195.7 °C). The sample was degassed at 200 °C for 2 h. The X-ray photoelectron spectroscopy (XPS) analysis was used to define the change in the surface chemical state of the samples before and after the reaction. The XPS investigation was conducted using a PHI 5000 VERSA PROBE III system equipped with a monochromatic Al Kα X-ray source operating at an energy of 1486.6 eV. Moreover, the gas chromatography (GC) technique was used to determine the composition of the product gas and the concentration of hydrogen produced during the chemical looping cycles. Analysis of the resultant gases generated during the reaction was conducted by using gas chromatography (GC).

2.3. OC Evaluation in the Batch-Fluidized Bed Reactor

An increased sample size in the fluidized bed reactor (FBR) allows for the examination of the gaseous products generated during the reduction and oxidation phases as well as the rate of mass loss caused by attrition, particle agglomeration, and carbon deposition on the particles. The FBR configuration comprises a quartz tube enclosed by an electric furnace, a cyclone separator for the selective separation of solid particles exiting the reactor, a condenser for the liquification of steam in the gas, a liquid–gas separator for the isolation of condensed liquid from gas, and a liquid storage container. The picture of the 3 kWh fluidized bed reactor used in this experiment is shown in Figure S1 (see Supporting Information).The gas analysis is conducted by connecting the liquid–gas separator to the gas chromatograph (GC). Furthermore, to accommodate looping processes, the FBR is linked to cylinders containing methane, air, and nitrogen. The comprehensive diagrams of the experimental setups are depicted in Figure . Prior to commencing the real experiment, the fluidization of the particles was performed using particles ranging from 150 to 200 μm. The increase in the gas flow rate led to a pressure difference between the reactor’s intake and output, which was recorded using a differential pressure transmitter (DPT) device installed in the reactor. For optimal fluidization, the gas flow rate at which DPT displays a constant value is selected. For COB particles with sizes between 150 and 200 μm, the experiment’s minimum fluidization velocity was found to be 1600 mL/min. The FBR experiment was conducted for 20 redox cycles at 750 °C, using a sample size of 10 g of OC and a gas flow rate of 1600 mL/min (50 Vol.% N2 and 50 Vol.% CH4/Air). The reaction temperature was fixed from the TGA experiments performed at two different temperatures in our previous work. TG plots of laterite ore (COB) reaction in the presence of CH4 during the heating stage and isothermal holding at 750 and 800 °C are shown in the Figure S2 (refer Supporting Information). During the heating stage, the mass loss in the laterite ore sample in the presence of CH4 is similar to that in the as-received laterite ore. However, in isothermal thermal holding at 750 °C, mass loss is observed only until the fourth minute of isothermal holding, and after that, an upward trend in the TG curve is observed. Similarly, in the reaction at 800 °C, mass loss was also observed in the heating stage, but in this case, mass gain was observed after the first minute of isothermal holding. This mass gain in the sample is attributed to carbon deposition on the sample. Carbon deposition on the sample can lead to poor OC performance, as Li et al. reported. Based on the TG results, the reduction temperature was fixed at 750 °C to avoid carbon deposition. The samples were maintained at 750 °C isothermally for the redox reaction in the FBR experiments. The reduction step was restricted to 27 min in the presence of CH4 as the reducing agent. In addition, the reduced OC undergoes reoxidation during the oxidation stage for a duration of 15 min. This process takes place in the presence of zero air (O2 + N2) as an oxidizing gas, which consists of 20% O2 in N2. The purpose of this is to decrease the reaction rate and regulate the reactor temperature as the oxidation reaction is very exothermic. An intermediate neutral phase is maintained for 15 min between the reduction and oxidation stages. During this time, N2 gas is continuously pumped through the reactor at a flow rate of 800 mL/min to eliminate any residual product gases and avoid any side reactions in the subsequent step. The gas produced by the reactor throughout the experiment was collected at every 2 min intervals and then analyzed using a NUCON gas chromatograph (GC) to determine the concentrations of the reactor output gases (CO, CO2, H2, CH4). A thermal conductivity detector (TCD) and a flame ionization detector (FID) were employed to capture the gas signals. The gas chromatograph (GC) was calibrated using standard gases, and a gas combination with a known composition was employed to quantify the product gases from the FBR. The output gas concentration data is utilized to calculate the concentration of H2, CO, CO2, and CH4, as well as the H2/CO ratio, in the product gases throughout the experiment, as a function of time in the redox cycles.

1.

1

Schematics of the fluidized bed catalytic reactor (FBR).

3. Results

Chemical composition of as-received COB samples obtained using the XRF technique is shown in Table . The composition study revealed that iron oxide makes up the majority of the COB sample’s makeup, along with oxides including Cr2O3, Al2O3, and SiO2. The as-received sample’s phase identification revealed the presence of quartz, chromite, and goethite phases in addition to a few hematite phase peaks. The presence of iron-containing phases is verified by both XRF and XRD investigation. In our previous study, a comprehensive investigation of phase transitions during the heating of COB in an inert environment is presented. Additionally, a thorough examination of the fluidized bed reactor’s multicycle redox experiment is presented in the following section. Furthermore, the next section also provides a comprehensive examination of gaseous products and reactive samples generated after various cycles.

1. Composition Analysis of the As-Received COB Sample.

composition Fe2O3 SiO2 Cr2O3 Al2O3 MgO NiO MnO CoO
weight (%) 80.6 5.73 5.53 4.51 1.25 0.94 0.82 0.13

3.1. OC Performance in the FBR

In order to identify the gases created during the cyclic reaction, samples of gaseous products formed during the reaction were collected and subjected to GC analysis. The results of the gas analysis conducted during the reduction cycles of the 1st, 5th, 10th, 15th, and 20th cycles are presented in Figure a–e. Gas sampling was conducted every 2 min during the isothermal holding phase of the reduction process. All cycles were subjected to gas analysis utilizing two detectors, namely TCD and FID. Based on the gas concentration graphs shown in Figure , it is evident that the quantities of H2 and CO show an upward trend with reaction time. The highest amounts were reached in 10 min during the first cycle. In the subsequent cycles, the maximum yield of H2 and CO was observed in between the 12th to 15th minute in the 5th, 10th, and 15th cycles. Subsequently, the quantities of H2 and CO decreased after the 15th minute and remained nearly constant until the conclusion of the reduction period up until 15th cycles. However, in the 20th cycle, the maximum H2 and CO yield was observed a little earlier in the 10th minute, and after that, the yield decreased and become constant until the end of the reduction period. Similarly, the H2/CO ratio during the first minutes of the first cycle reduction was close to the optimal H2/CO ratio value of 2. However, it decreased as time progressed and stayed constant after the sixth minute of the reaction. Nevertheless, in the case of other cycles, the H2/CO ratio remained consistently low below the optimal ratio for the entire reaction duration. The gas concentration analysis indicates that CO2 gas persists in the product gas until the fourth minute of reduction. In addition, it can be seen that the quantity of carbon monoxide (CO) produced in the following cycles exceeds the quantity of hydrogen (H2). The production of CO2 gas may be attributed to the initial total oxidation of methane gas within the first 4 min, followed by a transition to a partial oxidation process after the fourth minute, resulting in the generation of CO and H2 gases. Nevertheless, the CO2 level drops to minimal levels after the first four min, causing syngas to be produced. Moreover, the increase in the amount of CO in comparison to H2 can be due to the formation of carbon and its simultaneous reaction with other unreacted OC. The reason will be further elaborated in the subsequent section. Figure presents the reported total hydrogen yields in various cycles. After 20 redox cycles, the total H2 production from 10 g of COB is calculated to be 2736 mL. Moreover, the average H2/CO ratio in the first cycle was determined to be 1.48. Nevertheless, the ratio declined to 0.6, 0.75, 0.64, and 0.9 in the 5th, 10th, 15th, and 20th cycles, correspondingly, as depicted in Figure . The mean H2/CO ratio across 20 cycles was determined as 0.87. The data shown in Figure indicate that the H2 yield in the 20th cycle is lower than that in the 5th, 10th, and 15th cycles. The reduction in the amount of H2 and CO produced may be ascribed to the decline in the availability of lattice oxygen for the reaction caused by the development of a stable oxide layer with the increment in the number of cycles.

2.

2

Product gas concentration during the reforming reaction of methane in different cycles: (a) 1st cycle, (b) 5th cycle, (c) 10th cycle, (d) 15th cycle, and (e) 20th cycle.

3.

3

Total H2 yield and average H2/CO ratio in different cycles.

3.2. Characterization of Reacted OC

The phase identification of the reacted COB at the end of the 1st reduction period, 20th reduction period, and 20th oxidation period is shown in Figure . In the initial as-received samples, the XRD patterns matched with the goethite phase (PDF no. 01-078-8774), chromite phase (PDF no. 01-084-2811), and quartz phase (PDF no. 01-070-7344) majorly. At the end of the first reduction phase, the X-ray diffraction (XRD) investigation reveals the existence of the chromite phase (PDF number. 01-071-4917) with solubility of aluminum (Al) and magnesium (Mg), as well as the magnetite phase (PDF no. 01-071-6336). Furthermore, the study of the reaction product after the 20th reduction period revealed the existence of the chromite, magnetite, and forsterite phase. The existence of the magnetite/chromite phase in both the 1st and 20th reduction samples suggests that the OC material remains stable for 20 consecutive cycles. Moreover, the examination of the oxidized sample of the 20th cycle indicates that the magnetite/chromite phase remains in the sample following the reaction. In addition, the X-ray diffraction (XRD) pattern of the oxidized sample from the 20th cycle shows a smaller peak intensity of the hematite phase. This observation implies that as the number of redox cycles increases, only a limited quantity of magnetite undergoes transformation into fully complexed hematite in the oxidized samples. The decreased phase transformation may be ascribed to the reduced oxygen transport via the stable magnetite/chromite layer on the particle surface and the slower reaction kinetics during the conversion of hematite to magnetite phase. Further, the SiO2 (PDF no. 01-070-7344) peak at 20° and 25° in the unreacted sample disappears during the reaction and forms a ferrosilite (FeSiO3) phase (PDF no. 01-072-1509) observed at 26.4° and 44.3° in reacted samples obtained after the 1st reduction, 20th reduction, and 20th oxidation. Fe2O3, Cr2O3, MgO, MnO, and Al2O3 transform to form a spinel (chromite)­phase after the reduction reaction at 750 °C. This chromite phase remains stable throughout the 20 cycles. However, SiO2 present in the samples forms silicate phases with Fe and Mg during the redox reaction at 750 °C. This silicate phase does not react with methane. These inert phases provide stability to the oxygen carrier by preventing agglomeration of the active oxides and provide more surface area for better reaction. Similar observations for different inert materials have been reported in previous studies. −

4.

4

X-ray diffractogram of unreacted COB along with reacted samples after 1st reduction, 20th reduction, and 20th oxidation.

The particle surface morphology of the unreacted and reacted samples collected after 5th and 20th cycles is depicted in the SEM micrographs in Figure . As seen in Figure a, the surface morphology of the unreacted sample has a feathery and porous shape, indicating that the particle possesses a larger surface area. The surface morphology of reacted samples after 5th and 20th resembles a solid particle devoid of porosity, as shown in Figure b–d. Reacted samples exhibit the presence of particles with a regular form. In contrast, the unreacted samples have an uneven topography. The analysis of the surface micrographs of the unreacted samples (Figure a) indicates that a larger surface area and porous structure facilitated the reactions in the initial stages. Nevertheless, when the cycles increased, the surface area of the particles decreased, as seen in Figure b–d. BET analysis of the unreacted and reacted samples was performed to determine the pore volume and pore size. The results are reported in Table . According to the results, the pore size and pore volume of the reacted sample remain almost constant. It suggests that samples after multiple reactions maintain good stability without any sintering of pores. However, the H2 and CO yield decreases due to the formation of more magnetite and chromite phase with a decrease in the active Fe2O3 phase. Due to the thermodynamic limitation of the magnetite phase, deeper reduction of iron oxide is not feasible at 750 °C, causing a decrease in H2 and CO yield. Furthermore, there was no evidence of particle aggregation or particle breakage after 20 cycles. This observation implies that the COB particles exhibit strong resistance to agglomeration and attrition throughout extended redox cycles, therefore showing their excellent durability as an OC material.

5.

5

Surface morphology of the (a) unreacted sample, (b) oxidized sample after the 5th cycle, (c) oxidized sample after the 20th cycle, and (d) reduced sample after the 20th cycle.

2. BET Pore Size and Volume Analysis of Unreacted and Reacted COB Samples.

sample pore volume (cc/g) pore size (nm)
unreacted COB 0.0267 1.61
1 cycle (red) 0.0262 1.62
5 cycles (ox) 0.0203 1.60
20 cycles (red) 0.0269 1.62
20 cycles (ox) 0.0226 1.61

Microscopy images and analysis of the composition of the reacted COB sample after the oxidation reaction and the reduction reaction in the 20th cycle are shown in Figure and Tables S1 and S2. The samples’ micrographs from the 20th cycle reduction and 20th cycle oxidation reactions are shown in Figure a and b, respectively. Figure a displays the average composition of the oxidized sample obtained by EDS analysis. Points (1–3) indicate the existence of a chromite (FeCr2O4) type phase with a solubility of Al and Mg. The presence of the magnetite phase is also verified at points (4–8). An EDS study of points (9–13) shown in Table S1 (refer to the Supporting Information) reveals a minor amount of silicon in locations rich in iron and oxygen. This phase can be ascribed to the ferrosilite (FeSiO3) phase. Furthermore, Figure b displays the average composition analysis of reduced samples acquired after the 20th cycle. The point analysis presented in Table S2 (see the Supporting Information) confirms the presence of the chromite phase, magnetite, and ferrosilite (FeSiO3) phase. The phases reported in the EDS study of oxidized/reduced products at the conclusion of the 20th cycle match the XRD analysis. These findings suggest the presence of persistent magnetite/chromite phases in both oxidized and reduced samples. Furthermore, it confirms the partial reduction, which occurs with more cycles, because of the development of stable oxide phases and a decrease in the active oxide content.

6.

6

SEM micrograph of the reacted sample after the (a) 20th cycle (oxidized) and (b) 20th cycle (reduced).

This study used XPS analysis to assess the surface composition and chemical valence of COB in both its as-received and after-redox states for several cycles. Figure S3 displays the surface spectra of the as-received and reacted samples. The surface composition measurement in atomic percentages is represented in Table S3. All of the reacted samples had distinct Fe and O peaks, according to surface analysis data. The observation of an oxygen peak in the surface analysis of the reduced sample suggests the existence of stable oxide phases; this matches with the XRD and SEM-EDS analysis. Nevertheless, all the reacted samples also exhibited carbon peaks. This may be attributed to the carbon accumulation on the surface of the sample resulting from the decomposition of methane.

Figure summarizes the change in the chemical valence of Fe and Cr elements for the multicycle reacted and as-received samples. Figure a and b represent the separately corresponding spectra of Fe 2p and Cr 2p, respectively. The spectra of individual elements were fitted using the Gaussian approach and then stacked to analyze the variation in the oxidation status following several cycles. The fitted curve illustrates the peak locations of Fe 2p and Cr 2p before and after the reactions. The binding energy peak at 709.27 eV in the Fe 2p spectra of the as-received sample is attributed to Fe2+, whereas the peaks at 711.87 and 723.81 eV are attributed to Fe3+. , Upon evaluation of samples acquired after reduction in the 20th cycle, it is seen that Fe3+ peaks persist with Fe2+ peaks. The coexistence of Fe3+ peaks and Fe2+ peaks provides clear evidence for the development of the magnetite phase. Furthermore, it can be deduced that the majority of the active oxide undergoes conversion into a stable oxide, which limits the extent of reduction to a minimal level as the number of cycles increases.

7.

7

Individual element spectrum of (a) Fe 2p and (b) Cr 2p.

Furthermore, the Cr 2p spectra of the as-received sample may be separated into two peaks, namely, Cr 2p1/2 and Cr 2p3/2. These peaks can be further subdivided into Cr3+ peaks at 585.44/575.43 eV and Cr6+ peaks at 586.73/577.39 eV, respectively. Upon comparison of the Cr 2p spectra of the oxidized sample with the as-received sample, it is evident that the intensity of Cr3+ peaks increases in the first cycle. Nevertheless, the Cr6+ state is also detected after the first cycle as full reduction was not accomplished by the end of the first cycle period. Furthermore, in the oxidized sample of the 20th cycle, it is evident that the Cr6+ peak has undergone a total reduction in comparison to the Cr3+ peak. The existence of chromium in a trivalent form verifies the development of the chromite phase with higher cycles. The XPS analysis corroborates the results of XRD and SEM analyses in terms of phase formations as a function of reduction and oxidation cycles. In addition, the XPS analysis clearly elucidates the presence of Fe2+ in the reduced cycles, which is an indication of the sample undergoing reduction in the CH4 environment.

4. Discussion

The phase and composition analysis showed that COB is primarily an Fe-based material. It contains oxides of Fe along with other transition metal oxides (Cr2O3, MgO, and MnO) and inert oxides (Al2O3 and SiO2). According to the phase analysis of reacted samples shown in Figure , the formation of chromite and magnetite phase is observed after the reduction reaction in the 1st and 20th cycle. This result also corroborates with SEM-EDS analysis (see Figure ). Similarly, XPS analysis also revealed the presence of Fe in Fe2+ as well as in Fe3+ state, indicating the formation of magnetite after the reduction reaction. In addition, Cr3+ peaks in reacted samples confirmed the formation of a chromite phase. The reforming reaction of methane in the presence of COB can be expressed through reactions of methane and Fe oxide as mentioned below

4CH4+27Fe2O3→18Fe3O4+2CO2+2CO+3H2O+5H2 1

The formation of magnetite shows that reduction of Fe2O3 only proceeds until Fe3O4 at 750 °C according to reaction . Hence, the total conversion (reduction degree = R) of the OC during the redox reaction is calculated according to eqs and

6Fe2O3→4Fe3O4+O2 2
R=Δmoxygenmtotaloxygen 3

In this case, Δm (net change in amount of oxygen) is 2 and total oxygen is 18; therefore, the reduction degree is determined to be 11.11%.

In addition, one of the important aspects of an oxygen carrier is its oxygen storage capacity. The oxygen storage capacity of the OC is defined as the amount of oxygen that can be used in oxidizing the fuel (methane in this case). The oxygen storage capacity (R OC) is expressed by the equation mentioned

ROC=mo−mrmo 4

where m o and m r are the mass of oxidized and reduced sample, respectively.

The oxygen storage capacity of the COB is determined using thermogravimetry analysis. The details of TG analysis is reported in our previous work. According to the TG analysis, the average percentage of mass change in 20 cycles is 3.15%. This mass change can be correlated to the amount of oxygen released during the reduction reaction. Therefore, the oxygen storage capacity of COB as an OC material is 3.15% of the total mass. The phase analysis of the reacted COB samples suggests that the phase transition occurs only until magnetite (Fe3O4) from completely oxidized state (i.e., Fe2O3). According to the study of Cabello et al., the oxygen storage capacity between Fe2O3 and Fe3O4 is reported to be 2.1%. The oxygen storage capacity of COB is in good agreement with the reported value.

The reaction products of methane oxidation (reaction ) depend upon the amount of lattice oxygen available for the reaction. However, the abovementioned reaction of methane with OC taking place inside the reactor can be divided into three intermediate reactions, which are as follows: (1) decomposition of methane into carbon and hydrogen (reaction ), (2) reduction of Fe oxide by H2, CO, and C (reactions –), and (3) auxiliary reactions (reactions –). The detailed reactions involved in the looping process are expressed below:

4.1. Fuel Reactor

Step 1

CH4→C+2H2⁣ΔH°750°C=90kJ/mol⁣ΔG°750°C=−21.9kJ/mol 5

Step 2

Fe2O3+0.33H2→0.66Fe3O4+0.33H2O⁣ΔH°750°C=−2.4kJmol⁣ΔG°750°C=−28.9kJ/mol 6
Fe2O3+0.33C→0.66Fe3O4+0.33CO⁣ΔH°750°C=42.8kJ/mol⁣ΔG°750°C=−32.5kJ/mol 7
Fe2O3+0.33CO→0.66Fe3O4+0.33CO2⁣ΔH°750°C=−13.9kJ/mol⁣ΔG°750°C=−29.7kJ/mol 8

Step 3

H2O+CO→H2+CO2⁣ΔH°750°C=−34.5kJ/mol⁣ΔG°750°C=−2.39kJ/mol 9
H2O+C→H2+CO⁣ΔH°750°C=135.8kJ/mol⁣ΔG°750°C=−10.9kJ/mol 10
CO2+C→2CO⁣ΔH°750°C=170.4kJ/mol⁣ΔG°750°C=−8.49kJ/mol 11

4.2 Oxidation Reactor

Fe3O4+0.5O2→1.5Fe2O3⁣ΔH°750°C=−120.4kJ/mol⁣ΔG°750°C=−52.3kJ/mol 12

The gaseous products formed in the methane reforming reaction with COB particles can be explained by 3 intermediate reaction steps. First, the decomposition of methane occurs via reaction . This can occur on the particle surface as well as on the reactor wall (quartz tube). From the GC analysis shown in Figure , it can be noted that only 1–2 vol % out of 50 vol % CH4 is transformed to H2, CO, and CO2 at 750 °C. Since more than half of methane is present in the exist gas, the decomposition reaction has not achieved completion. Second, decomposed products then react with iron oxide present in the sample to form magnetite along with H2O, CO, and CO2 according to reactions , , and , respectively. That is why a small vol %. of CO2 is observed in the initial 4 min of each reduction cycle, as shown in Figure . In addition, the GC analysis also showed that the amount of H2 is less in comparison to that of CO in the product gas. The reason behind the lower amount of H2 could be attributed to the reduction reaction of the OC material with H2 as the reduction rate in H2 is higher in comparison to CO and C. The faster reaction rates of H2 can lead to the utilization of H2 formed in reaction . Further, the H2O and CO2 gases formed during step 2 passes through the particle bed and react with deposited carbon to form more CO and H2, according to reactions , , and . This increases the amount of CO in the product gas, leading to a decrease in the H2/CO ratio, as shown in Figure . A similar mechanism of methane conversion was also suggested in the DFT study by Feng et al. According to their study, the decomposition of methane begins with the adsorption of CH4 on the active sites of oxide particles followed by dehydrogenation. Further, the dehydrogenated products interact with surface oxygen to form CO, CO2, H2, and H2O. Their study reported that the formation of complete oxidized products is more favorable due to lower energy barriers for CO2(0.15 eV) and H2O­(1.17) generation in comparison to the generation of CO­(0.86 eV) and H2(2.51). However, in our study, the GC analysis clearly showed the generation of H2 and CO in majority due to the auxiliary reactions – occurring in the fluidized reactor.

Considering the abovementioned reactions involved in the reduction and oxidation of the OC material, the thermal balance of the whole process can be determined. This thermal balance of the process will suggest the endothermic or exothermic nature of the complete process. The thermal balance of an oxygen carrier (OC) in a chemical looping process is described by the net enthalpy change arising from all redox reactions that the OC experiences during both reduction and oxidation. The principal active component of chromite overburden (COB) utilized as an OC is Fe2O3. Consequently, the dominating reactions occurring during the reduction phase in the presence of methane (CH4) are outlined as reactions –, and the associated oxidation process is reported in reaction . The enthalpies of each of these reactions are determined at 750 °C. The cumulative enthalpy of the reduction reactions (reactions –) is ascertained to be +116.6 kJ/mol, whereas the enthalpy of the oxidation reaction (reaction ) is −120.4 kJ/mol. The net enthalpy change for the chemical looping process utilizing COB is −3.8 kJ/mol. The negative net enthalpy signifies that the process is marginally exothermic at 750 °C. Consequently, no external energy input is necessary to sustain the chemical looping reforming of methane with COB as the oxygen carrier.

The carbon deposition in the reaction and decrease in the H2–CO yield in higher cycles can be validated using thermodynamic calculations. To account for the different reaction products at 750 °C, thermodynamic calculations were performed using FactSage. In the calculations, methane was fixed to 1 mol, and the composition of COB was fixed on a 10 g basis. The calculation was performed with varying partial pressure of oxygen to replicate the reducing condition. The results of the thermodynamic calculations are shown in Figure . It can be seen that at partial pressure of oxygen lower than 1 × 10–21 atm, C is formed along with spinel (Fe3O4/FeCr2O4) and phase (Fe2SiO4). In addition, the H2 fraction in the gas phase increases, as well. This suggests that in excess CH4, and under extreme reducing conditions, carbon deposition is favored due to methane splitting. According to reactions and reported in Section , the ΔG at 750 °C of the C reaction with Fe2O3 (reaction ) is lower in comparison to the reduction of Fe2O3 with H2 (reaction ). Therefore, the reduction of Fe2O3 with C will be favored. The deposited carbon would react with other unreacted OC and form CO gas, leading to an increase in the CO concentration and a decrease in the H2/CO ratio with an increase in subsequent cycles.

8.

8

Thermodynamic calculation of methane reforming reaction with COB (a) volume fraction of gases, and (b) mole fraction of stable phases.

The total H2 yield reported in Figure increased until the 15th cycle, and then the value decreased in the 20th cycle. This could be attributed to multiple factors such as (1) decrease in the active sites for methane decomposition, and (2) decrease in oxygen diffusivity to the surface of the particle. A detailed schematics of the reaction mechanism in the FBR is given in Figure . Typically, the reduction process of a particle occurs in three stages: (1) formation of oxygen ions/vacancies, (2) mass transfer of oxygen ions via the core and product layer, and (3) surface reaction. The rate at which oxygen ions diffuse through the product layer determines the extent to which reduction occurs. The presence of a stable oxide will impede the movement of oxygen ions, leading to a decrease in the reactivity of the particle. In our case, the existence of components such as Cr, Mg, and Al facilitates the formation of a stable chromite spinel phase. By virtue of their high thermal stability, chromite spinel phases impede the movement of oxygen ions through the product layer and reduce the availability of active sites for methane decomposition. Consequently, it reduces the quantities of H2 and CO produced in the 20th cycle.

9.

9

Schematics of the methane reforming reaction mechanism.

A comparison of the total H2 yield of laterite ore (COB) obtained in the current study and the various complex metal oxide OCs − reduced in the presence of CH4 gas is shown in Figure below. The figure shows that the laterite (COB) sample yielded total hydrogen of 12.2 mmol/g of OC in 20 cycles compared to other complex oxygen carriers reported for only 5 or 10 cycles. In some cases, the H2 yield from the COB sample is even higher than the expensive metal oxide OCs, such as cerium oxide-based OCs, which are only reported for 5 redox cycles. Other low-cost oxygen carriers have also been tested in chemical looping processes, such as iron ore, manganese ores, ilmenite, and industrial wastes, such as mill scale and red mud. However, the experiments reported with these OCs have been performed at higher temperatures like 800–950 °C. The composition of reducing gas comprises a lesser amount of CH4 with steam or CO2, which is different from our experiment. For example, Araújo Barros do Nascimento Santiago et al. performed CLC experiments with Brazilian iron ore at 950 °C with a gas composition of (25% CH4, 10% H2O, 65% N2). Their results showed that complete oxidation of methane occurs in the reaction. The material exhibited no carbon deposition, minimal attrition loss, and a consistent lifespan of 15,000 h. In their study, they have not reported any H2 and CO yields for multiple cycles. Similarly, Condori et al. tested iron ore, manganese ore, and ilmenite as OCs for biomass gasification and syngas generation. They performed the reactions in the 800–950 °C temperature range with industrial wood pellets and pine wood. Their study showed a syngas yield of 0.6 N m3/kg biomass with Fe and Mn ore. Ilmenite also yielded 0.65 N m3/kg biomass with a gas composition of 37–40% CO2, 27–30% H2, 17–21% CO, 10–12% CH4, and 2–3% C2–C3. Their experiments have not reported the multicycle syngas yield. Therefore, comparing the yield of H2 and CO with the above-reported OCs is difficult due to their variation in experimental conditions.

10.

10

Comparison of the H2 yield using COB as an OC with other OCs.

Ores and mining/industrial waste use depend on their availability and cost. Materials like iron ore, manganese ore, ilmenite, and mining/industrial waste like red mud and COB are cheaply available as they do not find any commercial advantage. Huge amounts of these wastes are readily available, specific to a particular location. Moreover, all low-cost materials like iron ore, manganese ore, ilmenite, red mud, and COB contain a good amount of iron and other transition metal oxides, which can act as active oxide material for chemical looping reactions. H2 generation using COB will be cheaper than other synthetic OC materials as it is a mining waste. H2 yield comparison shows that COB can replace the complex metal oxide OCs in the chemical looping process and generate renewable and sustainable energy. Further, H2 and CO generated in the process can be implemented in sustainable development to achieve a low carbon footprint.

The performance of the oxygen carrier showed promising results in a 3 kWh fluidized bed reactor. According to the results of FBR experiments, COB can withstand multicycle redox reactions without deactivation of the sample due to sintering or carbon deposition. The analysis of the reacted samples in XRD and SEM-EDS showed the formation of stable oxide phases, contributing to material stability throughout 20 cycles. The total H2 yield in this 3 kWh fluidized bed reactor is 2736 mL for 10 g of sample in 20 cycles.

Further, 1–2 kg of COB samples can be tested in a bigger reactor to ascertain the OC performance on a bigger scale. Utilizing mining waste such as COB as an oxygen carrier on a bigger scale can complicate the process. The complexities may include variation in the composition of oxide, deactivation of the oxygen carrier, char formation, reactor design/heat management, improper fluidization, and carbon deposition. To ensure good performance of the OC and reactor, minimizing the process’s complexities is necessary. For example, the compositional variation in the oxygen carrier sample can be minimized by heating the sample in an oven to remove volatiles and moisture. Preoxidation of the sample can also be performed before cyclic reactions to ensure the samples are completely oxidized before reforming reactions.

Further, in industrial-scale applications, heat management of the process becomes a critical challenge due to the larger size of the reactor. In such systems, temperature gradients may form, leading to incomplete reactions. This problem can be avoided by preheating the reaction gas before entering the reaction chamber to minimize the temperature change in the reactor. Similarly, the functioning of the process is dependent on the degree of fluidization. Due to the more significant dimension of the reactor on a commercial scale, it becomes difficult to attain proper fluidization. So, to ensure better fluidization, the minimum fluidization velocity of the gas should be maintained, particle density and size should be predetermined so that it can be easily fluidized, and the bed height should be kept at an optimal height such that it can be fluidized easily. Computational methods such as computational fluid dynamics (CFD) simulation of the fluidized bed reactor can be performed to determine the flow rates, reactor heat management, particle bed height, and particle size for proper interaction. Ensuring the above points can establish the COB as an oxygen carrier in chemical looping reforming in larger-scale applications.

The experimental results showed that COB performed better than the other synthetic oxygen carriers. The hydrogen yield is comparable to that of Ce-based OCs. However, reforming reactions with COB showed limited reduction due to the formation of stable oxide phases, such as chromite and magnetite. This limits the hydrogen yield for longer cycles. The reaction performance can be improved by changing the physical and chemical properties of the OC. Doping of elements or inert support material, which effectively reduces the oxygen vacancy formation energy and oxygen diffusion energy, is considered to improve the redox performance of the OC primarily by enhancing the oxygen anion diffusivity. As a result, designing a metal oxide support matrix with high oxygen anion conductivity can create effective oxygen carrier particles with good reactivity and recyclability. In literature, it has been reported that adding inert phases like Al2O3, SiO2, TiO2, and ZrO2 improves the performance of the OC. In mining wastes like COB, the composition already has inert oxides like Al2O3 and SiO2, which will aid the stability of the material for multicycle reactions. However, higher amounts of Fe2O3 in the sample lead to carbon deposition, which affects the hydrogen yield. Therefore, to improve the hydrogen yield, the composition of COB can be modified by adding active oxides such as MnO, MgO, and CaO to restrict carbon formation and increase the hydrogen yield.

5. Conclusion

This study aimed to explore the use of chromite overburden, a mining waste, as an oxygen carrier in the chemical looping reforming of methane for the generation of syngas (H2 + CO) in a 3 kWh fluidized bed reactor. The high concentration of the iron oxide phase in COB makes it an appealing OC material. The following deductions are drawn from the experiment results:

  • 1.

    According to the surface morphology of the unreacted and reacted samples, no surface attrition or sample cracking were observed in higher cycles, suggesting good mechanical strength of the particles. In addition, COB particles did not show any sign of agglomeration in 20 cycles, indicating good agglomeration resistance property in longer cycles. Therefore, COB particles are ideal for the multicycle CLR process in fluidized bed reactors.

  • 2.

    The gas composition in the product gas analysis in GC showed the presence of H2, CO, and CO2. The formation of CO2 in the initial 4 min of reaction can be attributed to complete oxidation of methane due to the presence of a higher amount of lattice oxygen in the OC. Further, after the fourth minute, the CO2 concentration in the output gas becomes minimal and only partial oxidation of methane to H2 and CO occurs in the reaction. It was also observed that the amount of CO in the product gas was higher in comparison to H2. This could be because of the auxiliary reactions occurring due to carbon deposition. Further, gas analysis also indicated the reactions during the reduction reaction followed a 3-stage mechanism, i.e., decomposition of methane into carbon and hydrogen, reduction of Fe oxide by H2, CO, and C, and auxiliary reactions involving H2O, CO, CO2, and C.

  • 3.

    Phase characterization of the reacted samples using XRD and SEM from several cycles revealed the development of a persistent chromite and magnetite phase following the first oxidation reaction. This phase impedes the transport of oxygen to the surface of the particles in the lattice, resulting in incomplete reactions in the next cycles. The phase analysis showed an oxide conversion/reduction degree (Fe2O3 to Fe3O4) of 11.11% during the redox cycles.

The above-reported findings of the fluidized bed reactor experiments confirm that the transformation of Fe2O3 in the unreacted COB sample to chromite and magnetite in the reduction stage leads to the reforming of methane forming H2 and CO through partial oxidation. The study confirms COB’s suitability of COB as an oxygen carrier (OC) due to its high iron oxide content and strong mechanical stability, showing no attrition, cracking, or agglomeration over 20 cycles. Phase characterization indicated the formation of a persistent chromite phase after the first oxidation cycle, limiting oxygen transport and slightly reducing the reaction efficiency. Gas analysis revealed a three-stage reaction mechanism with initial complete methane oxidation followed by partial oxidation, favoring CO formation due to carbon deposition. Overall, COB achieved a total hydrogen yield of 2736 mL per 10 g OC, with an average H2/CO ratio of 0.87, proving its effectiveness in multicycle chemical looping reforming (CLR). Utilizing COB as an OC in chemical looping is a cost-effective method for the synthesis of syngas from mining waste. This approach also enables the development of renewable and sustainable energy. Future work will aim to modify the OC composition and perform redox cyclic tests to examine the cyclic performance of the redesigned oxygen carrier.

Supplementary Material

ao4c08878_si_001.pdf (261.4KB, pdf)

Acknowledgments

The authors would like to acknowledge the financial support provided by Ministry of mining (India), with the grant sanction number: SNTMOM/448/2021.

Glossary

Abbreviations

IPCC

Intergovernmental Panel on climate change

CLR

chemical looping reforming

OC

oxygen carrier

FBR

fluidized bed reactor

SEM

scanning electron microscopy

EDS

energy dispersive spectroscopy

XRD

X-ray diffraction

XRF

X-ray fluorescence

GC

gas chromatography

TCD

thermal conductivity detector

FID

flame ionization detector

The Supporting Information is available free of charge at https://pubs.acs.org/doi/10.1021/acsomega.4c08878.

  • 3 kWh fluidized bed reactor instrument, TG curves of laterite ore reduced in the presence of CH4 at 750 and 800 °C, surface scan of as-received laterite ore and reacted samples, EDS point analysis average composition of samples (oxidized) in the 20th cycle, EDS point analysis average composition of samples (reduced) in the 20th cycle, and surface composition of COB samples before and after reaction (PDF)

Swagat Das: Methodology, formal analysis, investigation, writingoriginal draft, and writingreview and editing. Manas Paliwal: Conceptualization and supervision.

The authors declare no competing financial interest.

References

  1. Calvin, K. , Dasgupta, D. , Krinner, G. , Mukherji, A. , Thorne, P. W. , Trisos, C. , Romero, J. , Aldunce, P. , Barrett, K. , Blanco, G. , Cheung, W. W. L. , Connors, S. , Denton, F. , Diongue-Niang, A. , Dodman, D. , Garschagen, M. , Geden, O. , Hayward, B. , Jones, C. , et al. IPCC, 2023: Climate Change 2023: Synthesis Report. Contribution of Working Groups I, II and III to the Sixth Assessment Report of the Intergovernmental Panel on Climate Change, Lee, H. ; Romero, J. , Eds. IPCC, Geneva, Switzerland. 2023. [Google Scholar]
  2. Das S., Biswas A., Tiwary C. S., Paliwal M.. Hydrogen production using chemical looping technology: A review with emphasis on H2 yield of various oxygen carriers. Int. J. Hydrogen Energy. 2022;47:28322. doi: 10.1016/j.ijhydene.2022.06.170. [DOI] [Google Scholar]
  3. Samprón I., de Diego L. F., García-Labiano F., Izquierdo M. T.. Effect of the Fe content on the behavior of synthetic oxygen carriers in a 1.5 kW biomass chemical looping gasification unit. Fuel. 2022;309:122193. doi: 10.1016/j.fuel.2021.122193. [DOI] [Google Scholar]
  4. Mattisson T., Keller M., Linderholm C., Moldenhauer P., Rydén M., Leion H., Lyngfelt A.. Chemical-looping technologies using circulating fluidized bed systems: Status of development. Fuel Process. Technol. 2018;172:1–12. doi: 10.1016/j.fuproc.2017.11.016. [DOI] [Google Scholar]
  5. Li X., Wang L., Zhang B., Khajeh A., Shahbazi A.. Iron oxide supported on silicalite-1 as a multifunctional material for biomass chemical looping gasification and syngas upgrading. Chem. Eng. J. 2020;401:125943. doi: 10.1016/j.cej.2020.125943. [DOI] [Google Scholar]
  6. Araújo Barros do Nascimento Santiago R., de Araújo Melo D. M., Adánez-Rubio I., Braga R. M., Adánez J., César Santiago R., Bezerra de Araújo Medeiros R. L.. Evaluation of Brazilian Iron-Based Ore and Industrial Waste as Low-Cost Oxygen Carriers for Chemical Looping Process. Energy Fuels. 2024;38:8168. doi: 10.1021/acs.energyfuels.4c00558. [DOI] [Google Scholar]
  7. Dilmaç N., Dilmaç O. ¨F., Yardımcı E.. Utilization of Menteş iron ore as oxygen carrier in Chemical-Looping Combustion. Energy. 2017;138:785. doi: 10.1016/j.energy.2017.07.126. [DOI] [Google Scholar]
  8. Zornoza B., Abad A., Mendiara T., Izquierdo M. T.. Iron-based oxygen carrier particles produced from micronized size minerals or industrial wastes. Powder Technol. 2022;396:637. doi: 10.1016/j.powtec.2021.11.016. [DOI] [Google Scholar]
  9. Adánez J., Condori O., de Diego L. F., Garcia-Labiano F., Izquierdo M. T., Abad A.. Syngas production in a 1.5 kWth biomass chemical looping gasification unit using Fe and Mn ores as the oxygen carrier. Energy Fuels. 2021;35:17182. doi: 10.1021/acs.energyfuels.1c01878. [DOI] [PMC free article] [PubMed] [Google Scholar]
  10. Condori O., García-Labiano F., de Diego L. F., Izquierdo M. T., Abad A., Adánez J.. Biomass chemical looping gasification for syngas production using ilmenite as oxygen carrier in a 1.5 kWth unit. Chem. Eng. J. 2021;405:126679. doi: 10.1016/j.cej.2020.126679. [DOI] [PMC free article] [PubMed] [Google Scholar]
  11. Shen X., Yan F., Zhang Z., Li C., Zhao S., Zhang Z.. Enhanced and environment-friendly chemical looping gasification of crop straw using red mud as a sinter-resistant oxygen carrier. Waste Manag. 2021;121:354. doi: 10.1016/j.wasman.2020.12.028. [DOI] [PubMed] [Google Scholar]
  12. Ganesh P., Dishwar R. K., Agrawal S., Mandal A. K., Sahu N., Sinha O. P.. Feasibility of nickel extraction from Indian chromite overburden by solid state reduction and smelting route. J. Min. Metall. Sect. B-Metall. 2020;56:229. doi: 10.2298/JMMB190908007G. [DOI] [Google Scholar]
  13. Das S., Biswas A., Bhattacharya J., Tiwary C. S., Paliwal M.. Utilization of laterite ore as an oxygen carrier in chemical looping reforming of methane for syngas production. Int. J. Hydrogen Energy. 2023;48:19411. doi: 10.1016/j.ijhydene.2023.02.054. [DOI] [Google Scholar]
  14. Li Y., Gong J., Huang F., Bai H., Wang F., Wang C.. Carbon Deposition and Sintering Characteristics on Iron-Based Oxygen Carriers in the Catalytic Cracking Process of Coal Tar. Energy Fuels. 2017;31:6501. doi: 10.1021/acs.energyfuels.7b00599. [DOI] [Google Scholar]
  15. Huang Z., Deng Z., Chen D., Wei G., He F., Zhao K., Zheng A., Zhao Z., Li H.. Exploration of Reaction Mechanisms on Hydrogen Production through Chemical Looping Steam Reforming Using NiFe2O4 Oxygen Carrier. ACS Sustain. Chem. Eng. 2019;7:11621. doi: 10.1021/acssuschemeng.9b01557. [DOI] [Google Scholar]
  16. de Caprariis B., Damizia M., De Filippis P., Bracciale M. P.. The role of Al2O3, MgO and CeO2 addition on steam iron process stability to produce pure and renewable hydrogen. Int. J. Hydrogen Energy. 2021;46:39067. doi: 10.1016/j.ijhydene.2021.09.135. [DOI] [Google Scholar]
  17. Hu Z., Miao Z., Wu J., Jiang E.. Nickel-iron modified natural ore oxygen carriers for chemical looping steam methane reforming to produce hydrogen. Int. J. Hydrogen Energy. 2021;46:39700. doi: 10.1016/j.ijhydene.2021.09.242. [DOI] [Google Scholar]
  18. Rai C., Bhui B., V P.. Techno-economic analysis of e-waste based chemical looping reformer as hydrogen generator with co-generation of metals, electricity and syngas. Int. J. Hydrogen Energy. 2022;47:11177. doi: 10.1016/j.ijhydene.2022.01.159. [DOI] [Google Scholar]
  19. McIntyre N. S., Zetaruk D. G.. X-ray Photoelectron Spectroscopic Studies of Iron Oxides. Anal. Chem. 1977;49:1521. doi: 10.1021/ac50019a016. [DOI] [Google Scholar]
  20. Tan B. J., Klabunde K. J., Sherwood P. M. A.. X-ray Photoelectron Spectroscopy Studies of Solvated Metal Atom Dispersed Catalysts. Monometallic Iron and Bimetallic Iron-Cobalt Particles on Alumina. Chem. Mater. 1990;2:186. doi: 10.1021/cm00008a021. [DOI] [Google Scholar]
  21. Desimoni E., Malitesta C., Zambonin P. G., Rivière J. C.. An x-ray photoelectron spectroscopic study of some chromium–oxygen systems. Surf. Interface Anal. 1988;13:173. doi: 10.1002/sia.740130210. [DOI] [Google Scholar]
  22. Monazam E. R., Breault R. W., Siriwardane R., Richards G., Carpenter S.. Kinetics of the reduction of hematite (Fe2O3) by methane (CH4) during chemical looping combustion: A global mechanism. Chem. Eng. J. 2013;232:478. doi: 10.1016/j.cej.2013.07.091. [DOI] [Google Scholar]
  23. Das S., Eden F., Paliwal M.. Syngas production through multi-cycle chemical looping of chromite mines waste: A sustainable approach to mitigate CO2 emissions. J. Cleaner Prod. 2023;420:138412. doi: 10.1016/j.jclepro.2023.138412. [DOI] [Google Scholar]
  24. Cabello A., Mendiara T., Teresa Izquierdo M., García-Labiano F., Abad A.. Energy use of biogas through chemical looping technologies with low-cost oxygen carriers. Fuel. 2023;344:128123. doi: 10.1016/j.fuel.2023.128123. [DOI] [Google Scholar]
  25. Ghosh D., Roy A. K., Ghosh A.. Reduction of Ferric Oxide Pellets With Methane. Trans. Iron Steel Inst. Jpn. 1986;26:186. doi: 10.2355/isijinternational1966.26.186. [DOI] [Google Scholar]
  26. Feng Y., Wang N., Guo X.. Reaction mechanism of methane conversion over Ca2Fe2O5 oxygen carrier in chemical looping hydrogen production. Fuel. 2021;290:120094. doi: 10.1016/j.fuel.2020.120094. [DOI] [Google Scholar]
  27. Zeng L., Cheng Z., Fan J. A., Fan L. S., Gong J.. Metal oxide redox chemistry for chemical looping processes. Nat. Rev. Chem. 2018;2:349. doi: 10.1038/s41570-018-0046-2. [DOI] [Google Scholar]
  28. Kang K. S., Kim C. H., Cho W. C., Bae K. K., Woo S. W., Park C. S.. Reduction characteristics of CuFe2O4 and Fe3O4 by methane; CuFe2O4 as an oxidant for two-step thermochemical methane reforming. Int. J. Hydrogen Energy. 2008;33:4560. doi: 10.1016/j.ijhydene.2008.05.054. [DOI] [Google Scholar]
  29. Cha K.-S., Yoo B.-K., Kim H.-S., Ryu T.-G., Kang K.-S., Park C. S., Kim Y. H.. A study on improving reactivity of Cu-ferrite/ZrO2 medium for syngas and hydrogen production from two-step thermochemical methane reforming. Int. J. Energy Res. 2010;34:422. doi: 10.1002/er.1643. [DOI] [Google Scholar]
  30. Kang K.-S., Kim C.-H., Bae K.-K., Cho W.-C., Kim W.-J., Kim Y.-H., Kim S.-H., Park C.-S.. Redox cycling of CuFe 2 O 4 supported on ZrO 2 and CeO 2 for two-step methane reforming/water splitting. Int. J. Hydrogen Energy. 2010;35:568. doi: 10.1016/j.ijhydene.2009.10.099. [DOI] [Google Scholar]
  31. Zhu X., Wang H., Wei Y., Li K., Cheng X.. Hydrogen and syngas production from two-step steam reforming of methane using CeO 2 as oxygen carrier. J. Nat. Gas Chem. 2011;20:281. doi: 10.1016/S1003-9953(10)60185-5. [DOI] [Google Scholar]
  32. Jeong H. H., Kwak J. H., Han G. Y., Yoon K. J.. Stepwise production of syngas and hydrogen through methane reforming and water splitting by using a cerium oxide redox system. Int. J. Hydrogen Energy. 2011;36:15221. doi: 10.1016/j.ijhydene.2011.08.079. [DOI] [Google Scholar]
  33. Zhu X., Wang H., Wei Y., Li K., Cheng X.. Reaction characteristics of chemical-looping steam methane reforming over a Ce – ZrO 2 solid solution oxygen carrier. Mendeleev Commun. 2011;21:221. doi: 10.1016/j.mencom.2011.07.017. [DOI] [Google Scholar]
  34. Zhu X., Wei Y., Wang H., Li K.. Ce e Fe oxygen carriers for chemical-looping steam methane reforming. Int. J. Hydrogen Energy. 2013;38:4492. doi: 10.1016/j.ijhydene.2013.01.115. [DOI] [Google Scholar]
  35. Zhao K., He F., Huang Z., Zheng A., Li H., Zhao Z.. Three-dimensionally ordered macroporous LaFeO3 perovskites for chemical-looping steam reforming of methane. Int. J. Hydrogen Energy. 2014;39:3243. doi: 10.1016/j.ijhydene.2013.12.046. [DOI] [Google Scholar]
  36. Zhu X., Wang H., Wei Y., Li K., Cheng X.. Hydrogen and syngas production from two-step steam reforming of methane. J. Rare Earths. 2010;28:907. doi: 10.1016/S1002-0721(09)60225-8. [DOI] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

ao4c08878_si_001.pdf (261.4KB, pdf)

Articles from ACS Omega are provided here courtesy of American Chemical Society

RESOURCES