Abstract
Despite numerous reports of an insulating ferromagnetic state in epitaxial LaCoO3 thin films, no consensus has been reached on the details of ferromagnetism in these films. To better understand the origins of magnetic order in such films, stoichiometric LaCoO3 films have been deposited on SrTiO3(001) and LaAlO3(001) substrates using off-axis sputtering. This technique allows growth to occur in conditions that minimize deviations from the ideal stoichiometry. SQUID magnetometry shows that ferromagnetism is stabilized only in films grown under tensile strain on SrTiO3. The magnetic properties of these films (T C ≈ 70 K, M sat ≈ 0.3 μB/Co, and H C ≈ 5 kOe) are essentially independent of thickness, consistent with nearly uniform magnetization. At room temperature, strain induced by the SrTiO3 substrate breaks the rhombohedral symmetry of the bulk structure, leading to a – a – c 0 octahedral tilting and an anisotropic distortion of the Co-centered octahedra. Low-temperature (T = 36 K) X-ray absorption spectroscopy reveals that tensile strain inherent to the SrTiO3 substrate stabilizes a substantial fraction of high- or intermediate-spin Co3+ ions, facilitating magnetic order, whereas films grown on LaAlO3 are made up nearly entirely of low-spin Co3+ ions.


1. Introduction
Among oxide perovskites, few compounds have been more intensively studied than LaCoO3. Interest in this compound is largely driven by the fact that Hund’s coupling, the energy scale associated with intra-atomic exchange, is comparable to the octahedral crystal field splitting of the d-orbitals of Co3+. Hund’s coupling favors electrons populating different orbitals with parallel spin, and therefore a high-spin (HS) configuration for Co3+ (t 2g 4 e g 2, S = 2), whereas crystal field splitting favors complete occupation of the t 2g orbitals, and therefore a nonmagnetic low-spin (LS) configuration (t 2g 6 e g 0, S = 0). The competition between these two states is such that the mixture of HS and LS Co3+ ions is sensitive to external perturbations, including temperature, pressure, and epitaxial strain. ,
The effects of temperature on the electronic, magnetic, and transport properties of bulk LaCoO3 have been extensively studied since the 1950s. The classic interpretation, first proposed by Goodenough, is that at low temperatures (T < 35 K) all Co3+ ions are in the LS state, save those ions near the surface, giving rise to a diamagnetic ground state. As the temperature increases the concentration of HS Co3+ rapidly increases at the expense of LS Co3+ until a 50:50 mixture of the two spin states is reached near 110 K. This situation persists until ∼350 K after which LS Co3+ ions are converted to intermediate-spin (IS) ions (t 2g 5 e g 1, S = 1) and the e g electrons start to delocalize. At still higher temperatures (T > 650 K) a homogeneous metallic state emerges. Subsequent studies tend to coalesce around a picture where all three spin statesHS, IS, LSplay a role in the temperature dependent magnetic and transport properties. , Nevertheless, the exact nature of the spin state transitions remains under debate, as some recent studies have suggested IS Co3+ does not play a prominent role and the spin states evolve directly from LS to HS.
Long range magnetic order is not observed in stoichiometric bulk samples. However, subtle perturbations that stabilize either HS or IS Co3+ ions at low temperatures can lead to a poorly understood ferromagnetic state. Weak ferromagnetism with a TC ≈ 85 K is well documented to occur in some bulk samples, even single crystals. This behavior is attributed to regions near the surface, where the coordination of cobalt ions is reduced to either tetrahedral or square pyramidal, thereby stabilizing the HS state. However, neither the details of the crystal structure nor the magnetic structure associated with the ferromagnetic regions are understood.
Even more intriguing is the stabilization of a “ferromagnetic” insulating state in epitaxial films grown on substrates that induce tensile strain. Since the initial discovery in 2007, this behavior has been reported by many different groups. − LaCoO3 films grown under 1–2% tensile strain exhibit Curie temperatures (T C) of 80–85 K, saturation magnetization (M sat) values of 0.5–1.2 μB/Co, and coercive fields (H C) of ∼5 kOe. Not surprisingly there are variations in properties from one study to another, with some reports show nonsaturating magnetization approaching 2 μB/Co. , A summary of the properties previously reported for LaCoO3 films can be found in the Supporting Information (Table S1).
While there is agreement that stabilization of a ferromagnetic insulating state requires a mixture of spin states, there is no consensus on the details of the magnetic ground state. Some researchers propose that ferromagnetism is stabilized by strain, others by defects, and still others by a combination of the two. Many studies of epitaxial LaCoO3 films report periodically repeating dark stripes in high-resolution transmission electron microscopy (HRTEM) images. Some early studies attributed these to extreme modulations of the Co–O bond distances that arise from stripe-like ordering of HS and LS Co3+ ions, but spatially resolved TEM imaging and electron energy loss spectroscopy show that the dark stripes arise from the presence of ordered oxygen vacancies. , Such defects create HS Co2+ ions (t 2g 5 e g 2, S = 3/2) which can play a pivotal role in stabilizing magnetic ordering. The similarity in the Curie temperatures of films grown under tensile strain (80–85 K) with the surface ferromagnetism seen in bulk samples (≈85 K) raises the possibility that oxygen vacancies might be playing an important role in the magnetism seen in thin films. In fact, some studies conclude that both strain and oxygen vacancy ordering act synergistically to stabilize ferromagnetism in films grown under tensile strain. ,
The overwhelming majority of LaCoO3 films studied to date have been grown using pulsed laser deposition (PLD). In a typical PLD growth the gas pressure is ∼150 mTorr and the substrate temperature is on the order of ∼700 °C. Both conditions are potentially problematic if one aspires to minimize deviations from the ideal stoichiometry. In those studies where the pressure inside the PLD chamber is varied, higher pressures lead to La-deficiencies on the order of 10%. , The relatively high temperatures needed for PLD growth of LaCoO3 films may be even more problematic. High temperatures favor the evolution of molecular oxygen and the reduction of Co3+ to Co2+. In-situ neutron powder diffraction studies of bulk LaCoO3 in a dynamic vacuum show that oxygen vacancy concentrations start to increase when the sample is heated above 525 °C, leading to the partial reduction of Co3+ to Co2+. While not identical to conditions used in thin film growth, there is good reason to believe that the conditions used for PLD growth encourage the formation of oxygen vacancies, leading to the presence of dark stripes seen in so many studies of LaCoO3 films.
In this paper, we utilize off-axis sputtering to grow LaCoO3 films on single crystal substrates that induce both compressive (LaAlO3) and tensile (SrTiO3) strain. Depositions are carried out at pressures (∼12 mTorr) and temperatures (∼450 °C) that are much lower than previous studies. By doing so we seek to minimize deviations from the ideal LaCoO3 stoichiometry and thereby disentangle the role of strain and defects on the magnetism of LaCoO3 films. This allows us to answer several questions about the intriguing and poorly understood magnetism of near-stoichiometric LaCoO3 films. For example, what pattern of octahedral tilting is induced by tensile strain? How do the Co–O bond distances and Co–O–Co bond angles respond to epitaxial strain, particularly tensile strain? How does strain impact the distribution of Co spin states? Can ferromagnetism be stabilized by strain alone and if so, how does it differ from the combined effects of strain and oxygen vacancies? Is the magnetically ordered state a simple colinear ferromagnet or is it a more complicated pattern of ordered spins?
2. Experimental Section
A polycrystalline LaCoO3 target was synthesized using conventional solid-state synthesis techniques. Stoichiometric amounts of La2O3 and Co3O4 were ball milled and then heated to 1150 °C for 48 h. The La2O3 was previously dried at 1000 °C for 12 h to prevent hydration. Phase purity was confirmed through X-ray powder diffraction (XRPD) on a Bruker D8 Advance powder diffractometer (40 kV, 40 mA, sealed Cu X-ray tube) equipped with a Lynxeye XE-T position-sensitive detector. The diffractometer is configured with an incident beam monochromator (Johansson type SiO2-crystal) that selects only Cu Kα1 radiation (λ = 1.5406 Å). The XRPD pattern of the polycrystalline target is shown in the Supporting Information (Figure S1). After pressing, the target was sintered at a temperature of 1108 °C for 2 h.
LaCoO3 thin film samples were grown by off-axis RF-sputtering. The operating pressure was fixed at 12 mTorr with an atmosphere that was 93% Ar and 7% O2. The optimal temperature window for growth was narrow and dependent on the choice of substrate. Films grown on SrTiO3(001) grew optimally at 450 °C while the optimal growth temperature on LaAlO3 substrates was 475 °C. The films were cooled from the growth temperature to room temperature at a rate of 20 °C/min in the same atmosphere used for deposition. X-ray diffraction (XRD) data on epitaxial films were taken using a Rigaku SmartLab operating in parallel beam mode with a Ge(220) double bounce monochromator. Samples were aligned to the (002) peak of the substrate, and symmetric 2θ-ω scans were performed around this range. Rocking curve measurements were performed using a Panalytical Empyreon with a Ge(220) four bounce monochromator combined with a triple bounce analyzer to achieve maximum angular resolution. Reciprocal space mapping (RSM) was performed with off-symmetric 2θ-ω scans around the (103) substrate peak using a Ge(220) four bounce monochromator and a two-dimensional detector. The thicknesses of the films were determined via X-ray reflectivity (XRR) measurements carried out with a Panalytical Empyreon and the data were fit to simulations to confirm thickness.
Density functional theory (DFT) calculations were performed using the Vienna Ab initio Simulation Package (VASP), with the Projector Augmented Wave (PAW) method. , The exchange-correlation functional was treated within the meta-generalized gradient approximation (meta-GGA) using the Regularized-Restored Strongly Constrained and Appropriately Normed (r2SCAN) formulation. A plane-wave energy cutoff of 550 eV was used, and the Brillouin zone was sampled using a gamma k-point spacing of 0.25 Å–1.
Scanning transmission electron microscopy was conducted to investigate the atomic structure with a probe-corrected Thermo Scientific Themis-Z STEM operated at 300 kV. The TEM thin foil was prepared via a FEI Helios NanoLab 600 DualBeam focus ion beam system. Nanodiffraction was performed using the Thermo Scientific Electron Microscope Pixel Array Detector.
Magnetization measurements on epitaxial films were carried out using a QuantumDesign MPMS3 operating in VSM mode. Samples were mounted for in-plane (IP) measurements with varnish and a quartz rod. Resistivity measurements were performed in a Dynacool Physical Property Measurement System (PPMS) from Quantum Design. Four-probe electrical measurements were carried out using a Keithley Model 2400 DC current source and a Keithley Model 2182 nanovoltmeter. The sample was patterned into a 10 × 40 μm bar, and a sensing current of 0.1 μA was applied.
X-ray absorption spectroscopy (XAS) measurements were performed at the SPEEM end-station of the UE49-PGMa beamline of BESSY II synchrotron radiation facility operated by Helmholtz-Zentrum-Berlin. Spectra of the Co L-edges were taken at 36 K to assess the spin states of cobalt at temperatures where magnetic ordering occurs (in films grown under tensile strain). Samples were capped with 0.5 nm platinum layer to prevent charging effects.
3. Results and Discussion
Epitaxial films of LaCoO3 with varying thicknesses were grown by off-axis sputtering on two perovskite substrates: SrTiO3 and LaAlO3. Substrate crystals were cut along the (001) face for a cube-on-cube growth. When grown on SrTiO3(001), LaCoO3 is under 2.0% tensile strain, whereas films grown on LaAlO3(001) are under 1.1% compressive strain. The XRD patterns of LaCoO3 films with various thicknesses grown on SrTiO3 can be seen in Figure a, with the rocking curve of the 35 nm LaCoO3 film shown in the inset. The full-width at half-maximum (fwhm) of the rocking curve, 0.0026°, is the narrowest reported to date for epitaxial LaCoO3 thin films. ,,,, Figure b shows similar results for films grown on LaAlO3. All films showed numerous Laue oscillations, indicating high quality crystal growths. The out-of-plane (OOP) lattice parameters for the films are plotted in Figure S2. The OOP lattice parameters qualitatively respond to strain as expected for both substrates. The tensile strain of the SrTiO3 substrate leads to a contraction of the OOP lattice parameter, while the compressive strain of the LaAlO3 substrate has the opposite effect. The films grown on SrTiO3 appear to be fully strained up to a thickness of 35 nm. For the films of 50, 60, and 80 nm thickness a small degree of strain relaxation can be observed, as indicated by the subtle increase of the OOP lattice parameter. The films grown on LaAlO3 do not show any obvious trend. The OOP lattice parameter averages to 3.869 Å.
1.

X-ray diffraction patterns of LaCoO3 films of various thicknesses grown on (a) SrTiO3(001) and (b) LaAlO3(001) substrates.
X-ray reciprocal space mapping (RSM) characterizes the distribution of scattered intensity in reciprocal space. Bragg peaks can determine crystal structure while satellite peaks and diffuse scattering indicate the presence of superlattices or in plane structural modulations. , RSM shown in the Supporting Information (Figure S3) confirm that our films are fully strained to the substrate. Scans along the pseudocubic [103] axis show no streaking or smearing of the film intensity relative to that of the SrTiO3 substrate in either the IP or OOP directions.
Experimental IP and OOP lattice parameters of the strained films are compared to the bulk in Table . Given the RSM results the IP lattice parameters are assumed to be equal to that of the substrate. Films under tensile strain from the underlying SrTiO3 substrate exhibit a unit cell volume (57.64 Å3) that is 2.7% larger than bulk LaCoO3, while films grown under compressive strain on LaAlO3 have a unit cell volume (55.56 Å3) that is 1.0% smaller. A more nuanced analysis using the Poisson ratio (estimated to be ν = 1/3 for LaCoO3) can be used to predict the OOP lattice parameter. Using this approach we see good agreement between the observed and expected OOP lattice parameter for films grown on LaAlO3, but the observed OOP lattice parameter for films grown on SrTiO3 (3.780 Å) is larger than predicted (3.753 Å). The anomalously large value of the OOP lattice parameter and unit cell volume for LaCoO3 films grown under tensile strain could be signaling an increase in the concentration of HS Co3+ (r = 0.61 Å) relative to the smaller LS Co3+ (r = 0.54 Å).
1. In-Plane (IP) and Out-of-Plane (OOP) Lattice Parameters for 17 nm Thick LaCoO3 Films Grown under Tensile Strain on SrTiO3 and Compressive Strain on LaAlO3 .
| bulk | epitaxial on LaAlO3(001) | epitaxial on SrTiO3(001) | |
|---|---|---|---|
| IP lattice parameter (Å) | 3.829 | 3.787 | 3.905 |
| OOP lattice parameter (Å) | 3.829 | 3.874 | 3.780 |
| unit cell volume (Å3) | 56.14 | 55.56 | 57.64 |
| Predicted OOP lattice parameter (Å) | 3.871 | 3.753 |
The predicted value of the OOP lattice parameter is calculated assuming a Poisson ratio ν = 1/3 given in reference .
The bulk lattice parameters represent a pseudocubic unit cell. A cubic unit cell with the same volume as the rhombohedral unit cell at 300 K. Values for the rhombohedral unit cell were taken from ref .
Next, we turn to the electrical transport and magnetic properties of the films. The insulating nature of the films was confirmed with temperature-dependent resistance measurements (Figure S4). Even when applying a current of 0.1 μA, the resistance below 180 K exceeded the limit of the instrument and could not accurately be measured. The magnetization vs applied field (M vs H) scans show that LaCoO3 films grown on SrTiO3(001) are clearly ferromagnetic at 5 K, as shown in Figure a. In contrast, the lack of either coercivity or remnant magnetization in the LaCoO3 films grown on LaAlO3(001) signal the absence of ferromagnetism, as shown in Figure S5. The nonlinear response and upturn in magnetization seen at low temperatures is likely the result of magnetic impurities in the LaAlO3 substrate. For the films grown on SrTiO3(001) the saturation magnetization is on the order of 0.3 μB per Co ion and the coercivity varies from 5–6 kOe for thinner films, increasing slightly for thicker films. The magnetization vs temperature (M vs T) scans show Curie temperatures ranging from 63 to 70 K (Figure b). Full details of the magnetism of each film grown on SrTiO3(001) are given in the Supporting Information (Table S2).
2.

(a) Magnetization vs applied field for various LaCoO3 films grown on SrTiO3(001). (b) Magnetization vs temperature for the same films.
The ferromagnetism seen in LaCoO3 films grown on SrTiO3 is broadly in agreement with prior studies (TC ≈ 85 K, HC ≈ 5 kOe, and Msat ≈ 1 μB/Co), though there are some notable differences. The ordering temperatures of our films are somewhat lower and the saturation magnetization is smaller by a factor of ∼3 with respect to most earlier studies. It is also noteworthy that the saturation magnetization, normalized per Co ion, does not vary systematically with changes in film thickness. This result excludes the possibility of ferromagnetism being confined to the interface or the free surface. Hence, we can rule out the possibility that the ferromagnetism seen here is the same as what is seen on the surfaces of bulk samples. Taken together with the minimal structural relaxation discussed above, the data strongly suggest that the observed ferromagnetism is relatively uniform throughout the film and driven primarily by the tensile strain imposed by the SrTiO3 substrate. Given our interest in understanding the ferromagnetic state, we focus primarily on films grown on SrTiO3 for the rest of this paper.
To assess the effect of strain on key bond distances and bond angles we turn to constrained DFT calculations. Bulk LaCoO3 has out-of-phase rotations/tilts of the octahedra about all three axes of the pseudocubic unit cell, which lower the symmetry from cubic to rhombohedral . This pattern of octahedral tilting, denoted as a – a – a –, can also be thought of as a single tilt about the cubic [111] axis. − The imposition of epitaxial strain breaks the degeneracy of the tilts about the pseudocubic axes and will necessarily lead to a change in the pattern of octahedral tilting. If tilting about the axis perpendicular to the substrate remains out-of-phase the tilt system becomes a – a – c – (space group C2/c). If it goes to zero the tilt system becomes a – a – c 0 (space group Imma). If it switches over to in-phase tilting the tilt system becomes a – a – c + (space group Pnma). Chaturvedi et al. carried out DFT calculations to compare the energies of various patterns of octahedral tilting as a function of epitaxial strain. They found that all three of the above tilt systems are nearly degenerate when the tensile strain exceeds ∼1%. They went onto conclude that a – a – c + tilting and Pnma symmetry is the most stable pattern for films grown on SrTiO3 (2.0% tensile strain) but conceded that other tilt systems could easily be stabilized at finite temperatures.
To explore the effects of tensile strain on the crystal structure, we started from a 2ap × 2ap × 2ap pseudocubic unit cell with atomic coordinates that correspond to the bulk rhombohedral structure and lattice parameters that are constrained in the ab-plane to match those of SrTiO3 (a = b = 2 × 3.905 Å = 7.810 Å), while the out-of-plane lattice constant and atomic coordinates were relaxed until the Hellman–Feynman on all atoms were reduced below 10 meV/Å. No symmetry other than translational symmetry was imposed on the structure. Non–spin-polarized calculations were chosen to focus on the coupling between the crystal structure, electronic structure, and epitaxial strain without the influence of spin degrees of freedom, as no long-range spin state ordering is expected near room temperature.
The geometry optimized structure is shown in Figure . The c-axis lattice parameter was optimized to a value of 7.511 Å, which reduces to 3.755 Å when converted to the smaller pseudocubic unit cell. This value is very close to the value of 3.753 Å predicted using Poisson ratio, but somewhat smaller than the 3.78 Å value seen experimentally. Nevertheless, it does qualitatively capture the contraction of the structure in the direction perpendicular to the substrate. A closer look at Figure reveals out-of-phase tilts about both the a- and b-axes, and no tilting around the c-axis, corresponding to the a – a – c 0 pattern of tilting. If we perform a symmetry reduction the structure can be written with Ibmm symmetry (a nonstandard setting of Imma) and a unit cell that is half the volume of the 2ap × 2ap × 2ap unit cell (Table S3).
3.

DFT-optimized structure of LaCoO3 grown in tensile strain on SrTiO3(001). (a) Perspective view with La, Co, and O shown as green, blue, and red spheres, respectively, viewed looking down the (b) c-axis showing the absence of octahedral tilts, (c) the b-axis showing out-of-phase tilts, and (d) the a-axis showing out-of-phase tilts. (e) An illustration of Co–O distances and Co–O–Co angles.
The pertinent bond distances and angles are shown in Figure e. Here we can see the effects of the tensile strain on the structure. Compared to the bulk values for the Co–O distance (1.935 Å) and Co–O–Co angle (163.7°), we see that the in-plane Co–O bonds have expanded (1.970 Å) and the Co–O–Co angle has slightly increased (165°). In contrast, the out-of-plane Co–O bonds have contracted (1.912 Å) and the Co–O–Co angle has become more acute (158°). This structure reveals the microscopic changes that lead to the observed in-plane expansion and out-of-plane contraction of the unit cell. In hindsight, the lack of tilting around the c-axis is not surprising. Such tilting, either in-phase or out-of-phase, would effectively decrease the lattice parameters in the ab-plane, which would exacerbate the mismatch with the SrTiO3 substrate.
High-resolution STEM was employed to investigate the effects of tensile strain on the atomic structure of LaCoO3. Figure a presents a high-angle annular dark field (HAADF) micrograph of the 35 nm-thick LaCoO3 film grown on the SrTiO3(001) substrate, viewed along the [100]c zone axis (indexed in the pseudocubic system). The micrograph reveals a remarkably sharp and coherent heterointerface between the film and substrate, with no observable interfacial secondary phases or structural defects. Thus, demonstrating the excellent crystalline quality and epitaxial registry of the film grown using our optimized off-axis RF-sputtering technique. The uniform atomic arrangement within the LaCoO3 layer further confirms the high structural integrity and reproducibility of the growth process.
4.

(a) HAADF micrograph of the LaCoO3(35 nm)/SrTiO3(001) film viewed from the [100]c-zone axis, indexed with a pseudocubic unit cell. Nanodiffraction patterns were acquired from the circled regions. Area b corresponds to SrTiO3 and area d to LaCoO3. The measured ratio of distances, k z /k y , between the (001) and (010) reflections relative to the direct reflection (000), is 1.001, for SrTiO3 and 1.029 for LaCoO3. (c) The simulated SrTiO3 diffraction pattern, yielding theoretical k z /k y ratio of 1.000. (e–g) Simulated LaCoO3 diffraction patterns for structures with (e) Pnma, (f) Imma, and (g) C2/c symmetry. The scales in Figure b–g are identical; for simplicity, one scale bar corresponding to 2 nm–1 is shown in Figure f.
In contrast to previous reports on LaCoO3 films fabricated by high-pressure PLD, where vertical “dark stripe” features are often observed along the [100]c zone axis, , our sputtered films do not exhibit such stripes, consistent with a stoichiometric composition and the absence of long-range ordered defects. This observation underscores a key advantage of the RF-sputtering approach, which provides control over the stoichiometry that is superior to PLD, at least for the growth of LaCoO3 films.
To further elucidate the precise crystal symmetry, nanodiffraction experiments were subsequently performed on Area b (SrTiO3 substrate) and Area d (LaCoO3 film) in Figure a. The resulting experimental diffraction patterns, shown in Figure b,d, are systematically compared with simulated patterns in Figure c,e–g, representing SrTiO3 and potential LaCoO3 structures with Imma, Pnma, and C2/c space group symmetry, all viewed along the [100]c-zone axis. The Imma structure was obtained from the DFT calculations discussed above. The Pnma structure was obtained using the structure prediction software SPuDS with lattice parameters adjusted to match the Imma structure, and the C2/c structure was taken from the literature. The comparison between the simulated and experimental patterns was conducted in terms of ratio of reciprocal spacings, k z /k y , between the (001) and (010) reflections relative to the central (000) transmitted beam. The experimental value for the SrTiO3 substrate, 1.001, agrees exceptionally well with the expected value of 1.000 for a cubic perovskite, validating the reliability and accuracy of our diffraction analysis. The measured k z /k y ratio of 1.029 for LaCoO3 closely matches the value of 1.032 derived from the DFT calculations for the orthorhombic Imma space group (a – a – c 0 tilt system), and the k z /k y ratio of 1.033 calculated from the XRD lattice parameters. (Note that the reciprocal space k z /k y is just the inverse of the real space c/b.)
The alternative orthorhombic structure with Pnma symmetry and a – a – c + tilting, is differentiated from the Imma structure by {eeo} (even, even, odd)-type superlattice reflections arising from in-phase octahedral rotations along the c-axis (Figure e). Crucially, such reflections are not observed in the experimental diffraction pattern, Figure d, thereby allows us to exclude this space group from consideration. Although the electron diffraction patterns of the Imma (a – a – c 0 tilts) and C2/c (a – a – c – tilts) structures have the similar diffraction spots in this projection, other factors argue in favor of adoption of the former tilt system. First, out-of-phase tilts about the axis perpendicular to the substrate are allowed in our DFT calculations, but the geometry optimized structure indicates that those tilts go to zero. Second, if there were substantial tilts about the c-axis it would reduce the length of the a and b lattice constants pushing the c/b (and c/a) ratio toward unity, contrary to the findings of both electron and X-ray diffraction measurements.
Further unambiguous confirmation of the Imma symmetry was obtained through integrated differential phase contrast (iDPC) imaging, as shown in Figure . The LaCoO3/SrTiO3(001) film was viewed along the [110]c-zone axis, and HAADF and iDPC micrographs were acquired simultaneously. Owing to their distinct contrast mechanisms (Z-contrast for HAADF and nearly linear contrast for iDPC), the lighter oxygen columns are more clearly visualized in the iDPC micrograph. The DFT-optimized Imma crystal structure model, overlaid across both the HAADF and iDPC images, shows excellent agreement with the experimentally observed atomic arrangement, providing compelling visual confirmation of the structural model.
5.

Composite HAADF (left) and iDPC (right) micrographs of the LaCoO3 (35 nm) film on the SrTiO3(001) substrate, viewed along the [110]c-zone axis. The HAADF and iDPC images were acquired simultaneously from the same region; the left half displays the HAADF signal and the right half the iDPC signal. A simulated Imma LaCoO3 structural model, corresponding to the DFT-optimized a – a – c 0 oxygen octahedral tilting system, is overlaid across both panels, with La, Co, and O atoms represented by green, blue, and red spheres, respectively.
The presence of ferromagnetism or any other type of cooperative magnetism in LaCoO3 films requires a non-negligible concentration of magnetic ions at low temperatures. Such behavior differs from bulk LaCoO3 where the ground state is made up almost exclusively nonmagnetic LS Co3+ (S = 0) ions. The magnetic ions could be HS Co3+ (S = 2), IS Co3+ (S = 1), or if oxygen vacancies are present HS Co2+ (S = 3/2). To investigate this aspect directly, synchrotron X-ray absorption spectra (XAS) at the Co L2 and L3 edges were collected at 36 K for 10 nm films grown on both SrTiO3 and LaAlO3. In bulk samples spectra collected at this temperature are dominated by LS Co3+ at this temperature, so the detection of other spin states and/or oxidation states can be directly attributed to the effects of strain or defects, or a combination of the two.
Figure a compares XAS measurements on LaCoO3 films grown on both SrTiO3 and LaAlO3 with several reference spectra where the spin state and oxidation state are well-defined. HS Co3+ has a distinctive pre-edge peak, labeled A, while LS Co3+ has a distinctive postedge feature labeled by peak B. The peak located near 777 eV (labeled C) is a pre-edge feature associated with HS Co2+. Notably, no features that can be attributed to Co2+ are seen in either film, further supporting our assertion that the concentration of oxygen vacancies is minimal. While the spectra for the films grown on SrTiO3 and LaAlO3 are similar, there are clear differences, as highlighted in the top panel of Figure b. The film grown on LaAlO3 has a pronounced shoulder on the high-energy side of the L3 peak, as would be expected if LS Co3+ is the dominant spin state. The film grown on SrTiO3 has a less prominent shoulder on the high energy side and greater intensity on the low-energy side of the peak. Both features that would be expected if some LS Co3+ ions are converted into HS Co3+.
6.

X-ray absorption spectra for (a) the Co L2 and L3 edges for various Co-containing oxides, taken from ref . The A label marks the pronounced low energy shoulder for HS Co3+, B marks the high-energy shoulder for LS Co3+, and C marks the lowest energy feature for Co2+. (b) The Co L3 XAS spectra taken at 36 K for LaCoO3 films grown on SrTiO3 and LaAlO3. Simulated fits to the data for a LaCoO3 film on LaAlO3 and SrTiO3. Details of the fits are given in the text.
In the bottom two panels of Figure b the experimental XAS data for these films are fit to simulations obtained from multiplet theory calculations. , The fits were obtained by taking a linear combination of LS Co3+ and either HS Co3+ or IS Co3+ spectra. These simulations were produced using CTM4XAS and an 80% Slater integral reduction with 10Dq = 2.0 eV for the HS and IS states and 2.2 eV for the LS state. The IS state is differentiated from the HS state by applying additional crystal field parameters associated with D 4h symmetry, D t = 0.04 eV and D s = 0.07 eV. The resulting simulations were broadened using a Lorentzian-Fano line shape and slightly energy shifted to match the experimental spectra.
The fitting indicates that the films grown on LaAlO3 contain predominantly LS Co3+ and thus are relatively insensitive to whether the magnetic ions are modeled as HS or IS Co3+. When fit assuming a mixture of LS and HS ions the modeling indicates that the films contain 98(5)% LS Co3+ and 2(5)% HS Co3+. When fit assuming a mixture of LS and IS the numbers change slightly to 95(6)% LS Co3+ and 5(6)% IS Co3+. In either case, the concentration of magnetic Co3+ ions is within one standard deviation from zero, and the fits are indistinguishable.
The fitting yields quite different results for LaCoO3 grown on SrTiO3. If we assume a mixture of LS and IS ions, as might be stabilized by the axial compression of the octahedra revealed by the DFT calculations, the best fit is obtained for a mixture of 62(6)% LS Co3+ and 38(6)% IS Co3+. If we fit the spectrum with a mixture of LS and HS Co3+ ions the concentration of magnetic HS Co3+ ions is reduced to 27(6)%, with a comparable quality of fit. Within the constrained variable approach used to fit the spectra, it is not possible to definitively say whether the film contains a mixture of LS and HS ions, a mixture of LS and IS ions, or possibly a mixture of all three spin states. However, we can say with certainty that films grown on SrTiO3 contain a non-negligible, but minority, fraction of either HS or IS ions, unlike films grown on LaAlO3.
Simple logic dictates that a mixture of spin states is needed to stabilize an insulating ferromagnetic ground state. If all Co3+ ions were to adopt a HS state the superexchange interactions between neighboring ions would be antiferromagnetic and the magnetic structure would be a G-type antiferromagnet, similar to LaFeO3. If the Co3+ ions were exclusively in an IS state, various pattens of orbital ordering could lead to some degree of local ferromagnetic coupling, as seen in LaMnO3, but an overall antiferromagnetic ground state is still the most likely outcome. Fujioka et al. proposed a ferrimagnetic arrangement of IS and HS Co3+ in a 3:1 ratio for films grown on LSAT substrates (T C = 94 K, M sat ≈ 0.7 μB/Co). While we cannot rule out that such a model could be applicable to the films they studied, the absence of LS Co3+ assumed in their model is clearly inconsistent with the XAS data collected here. Even a rock salt ordering of a 1:1 mixture of LS and HS Co3+ ions would be expected to stabilize an antiferromagnetic ground state, as seen for double perovskites like Sr2CoWO6. Therefore, an ordered pattern of HS and LS ions, where the magnetic HS ions make up <50% of the total Co3+ ions, seems the most promising way to stabilize an insulating ferromagnetic ground state. The challenge going forward is to identify the pattern of spin-state ordering that is consistent with ferromagnetic ordering, either by employing experimental probes to determine the arrangement of spin states at low temperatures and/or computational studies with large supercells that permit complex patterns of spin-state ordering.
The observation of a saturation magnetization on the order of ∼0.3 μB raises some doubts about the assumption often made in the literature that the ground state is a collinear ferromagnet. A HS Co3+ ion would have 4 unpaired electrons a local moment that is ∼4 μB. If all such moments were to adopt a colinear, ferromagnetic arrangement, the fraction of HS Co3+ ions would need to be <10% of the total number of cobalt ions to give saturated magnetization values comparable to those observed in this study. It is hard to believe that such a dilute array of magnetic ions would have sufficiently strong superexchange coupling to stabilize magnetic ordering at temperatures ranging from 60–80 K. This suggests the magnetic ground state may be more complicated than a simple collinear ferromagnet. Possibilities include noncollinear magnetism, ferrimagnetism, or inhomogeneous magnetism, although the latter would seem to be inconsistent with our magnetic and structural data that shows little dependence on film thickness.
4. Conclusions
Epitaxial LaCoO3 films with thicknesses varying from 10 to 80 nm have been deposited using off-axis RF-sputtering. Ordered planes of oxygen vacancies, commonly observed in PLD grown films, are not observed in high-resolution TEM images, and no sign of Co2+ is seen in XAS spectra, confirming that the composition of these films approaches the ideal LaCoO3 stoichiometry. The effect of tensile strain on the structure is to break the rhombohedral symmetry and distort the symmetric octahedra of bulk LaCoO3. Films grown on SrTiO3 substrates exhibit a – a – c 0 octahedral tilting, orthorhombic Imma symmetry, and an axial compression of the Co-centered octahedra. XAS measurements performed at low temperature (36 K) show that films grown on SrTiO3 have a mixture of HS and LS Co3+ ions or IS and LS Co3+ ions. In contrast, films grown on LaAlO3 contain little if any HS Co3+ (similar to bulk LaCoO3). The strain-induced change in the distribution of spin states explains in part why tensile strain stabilizes long-range magnetic order.
While the observation of low temperature ferromagnetism on films grown on SrTiO3 substrates is consistent with earlier studies of PLD-grown films, the saturation magnetization of the films studied here, ∼0.3 μB/Co, is smaller than most literature reports by a factor of ∼3. This reduction in magnetic moment is significant for two reasons. First, it infers that strain and oxygen vacancies work synergistically to enhance the ferromagnetism observed in many LaCoO3 thin films. Second, the size of the moment found here is inconsistent with a simple ferromagnetic alignment of the moments on the HS Co3+ ions, implying a more complicated low temperature magnetic structure.
Supplementary Material
Acknowledgments
This work was primarily supported by the Center for Emergent Materials (CEM), a National Science Foundation MRSEC under NSF Award Number DMR-2011876. The XRD and SQUID measurements were performed at the OSU NanoSystems Laboratory (NSL). Electron microscopy was performed at the Center for Electron Microscopy and Analysis (CEMAS) at The Ohio State University. Computational resources were provided by the Ohio Supercomputer Center. The authors thank the Helmholtz-Zentrum Berlin for the provision of access to synchrotron radiation facilities and allocation of synchrotron radiation at the SPEEM end-station of UE49-PGMa beamline.
The Supporting Information is available free of charge at https://pubs.acs.org/doi/10.1021/acs.chemmater.5c03290.
Review of literature reports of the magnetic properties of tensile strained LaCoO3 films; powder XRD for LaCoO3 sputter target; out-of-plane lattice parameters measured by XRD for films of varying thickness grown on SrTiO3 and LaAlO3 substrates; reciprocal space mapping of LaCoO3 films; electrical resistance as a function of temperature; magnetic measurements on films grown on LaAlO3 substrates; a summary of magnetic properties measured for LaCoO3 films grown on SrTiO3 substrates; and the crystallographic details of the DFT-optimized structure of LaCoO3 grown on SrTiO3 (PDF)
The authors declare no competing financial interest.
References
- Yan J. Q., Zhou J. S., Goodenough J. B.. Bond-length fluctuations and the spin-state transition in LCoO3 (L = La, Pr, and Nd) Phys. Rev. B. 2004;69:134409. doi: 10.1103/PhysRevB.69.134409. [DOI] [Google Scholar]
- Abbate M., Fuggle J. C., Fujimori A., Tjeng L. H., Chen C. T., Potze R., Sawatzky G. A., Eisaki H., Uchida S.. Electronic structure and spin-state transition of LaCoO3-II. Phys. Rev. B. 1993;47:16124. doi: 10.1103/PhysRevB.47.16124. [DOI] [PubMed] [Google Scholar]
- Goodenough J. B.. An interpretation of the magnetic properties of the perovskite-type mixed crystals La1–xSrxCoO3−δ . J. Phys. Chem. Solids. 1958;6:287–297. doi: 10.1016/0022-3697(58)90107-0. [DOI] [Google Scholar]
- Senaris-Rodriguez M. A., Goodenough J. B.. LaCoO3 Revisited. J. Solid State Chem. 1995;116:224–231. doi: 10.1006/jssc.1995.1207. [DOI] [Google Scholar]
- Saitoh T., Mizokawa T., Fujimori A., Abbate M., Takeda Y., Takano M.. Electronic structure and temperature-induced paramagnetism in LaCoO3 . Phys. Rev. B. 1997;55:4257. doi: 10.1103/PhysRevB.55.4257. [DOI] [Google Scholar]
- Radaelli P. G., Cheong S. W.. Structural phenomena associated with the spin-state transition in LaCoO3 . Phys. Rev. B. 2002;66:094408. doi: 10.1103/PhysRevB.66.094408. [DOI] [Google Scholar]
- Podlesnyak A., Streule S., Mesot J., Medarde M., Pomjakushina E., Conder K., Tankaka A., Haverkort M., Khomskii D.. Spin-state transition in LaCoO3: Direct neutron spectroscopic evidence of excited magnetic states. Phys. Rev. Lett. 2006;97:247208. doi: 10.1103/PhysRevLett.97.247208. [DOI] [PubMed] [Google Scholar]
- Yan J. Q., Zhou J. S., Goodenough J. B.. Ferromagnetism in LaCoO3 . Phys. Rev. B. 2004;70:014402. doi: 10.1103/PhysRevB.70.014402. [DOI] [Google Scholar]
- Fuchs D., Pinta C., Schwarz T., Schweiss P., Nagel P., Schuppler S., Schneider R., Merz M., Roth G., v. Löhneysen H.. Ferromagnetic order in epitaxially strained LaCoO3 thin films. Phys. Rev. B. 2007;75:144402. doi: 10.1103/PhysRevB.75.144402. [DOI] [Google Scholar]
- Freeland J. W., Ma J. X., Shi J.. Ferromagnetic spin-correlations in strained LaCoO3 thin films. Appl. Phys. Lett. 2008;93:212501. doi: 10.1063/1.3027063. [DOI] [Google Scholar]
- Mehta V., Biškup N., Jenkins C., Arenholz E., Varela M., Suzuki Y.. Long-range ferromagnetic order in LaCoO3−δ epitaxial films due to the interplay of epitaxial strain and oxygen vacancy ordering. Phys. Rev. B. 2015;91:144418. doi: 10.1103/PhysRevB.91.144418. [DOI] [Google Scholar]
- Biškup N., Salafranca J., Mehta V., Oxley M., Suzuki Y., Pennycook S., Pantelides S., Varela M.. Insulating ferromagnetic LaCoO3−δ films: A phase induced by ordering of oxygen vacancies. Phys. Rev. Lett. 2014;112:087202. doi: 10.1103/PhysRevLett.112.087202. [DOI] [Google Scholar]
- Choi W. S., Kwon J. H., Jeen H., Hamann-Borrero J. E., Radi A., Macke S., Sutarto R., He F., Sawatzky G. A., Hinkov V., Kim M., Lee H. N.. Strain-induced spin states in atomically ordered cobaltites. Nano Lett. 2012;12:4966–4970. doi: 10.1021/nl302562f. [DOI] [PubMed] [Google Scholar]
- Yoon S., Gao X., Ok J. M., Liao Z., Han M. G., Zhu Y., Ganesh P., Chisholm M. F., Choi W. S., Lee H. N.. Strain-Induced Atomic-Scale Building Blocks for Ferromagnetism in Epitaxial LaCoO3 . Nano Lett. 2021;21:4006–4012. doi: 10.1021/acs.nanolett.1c00756. [DOI] [PubMed] [Google Scholar]
- Kwon J. H., Choi W., Kwon Y., Jung R., Zuo J., Lee H., Kim M.. Nanoscale spin-state ordering in LaCoO3 epitaxial thin films. Chem. Mater. 2014;26:2496–2501. doi: 10.1021/cm5003115. [DOI] [Google Scholar]
- Fujioka J., Yamasaki Y., Doi A., Nakao H., Kumai R., Murakami Y., Kawasaki M., Arima T., Tokura Y.. Strain-sensitive spin-state ordering in thin films of perovskite LaCoO3 . Phys. Rev. B. 2015;92:195115. doi: 10.1103/PhysRevB.92.195115. [DOI] [Google Scholar]
- Li D., Wang H., Li K., Zhu B., Jiang K., Backes D., Veiga L. S. I., Shi J., Roy P., Xiao M., Chen A., Jia Q., Lee T. L., Dhesi S. S., Scanlon D. O., MacManus-Driscoll J. L., van Aken P. A., Zhang K. H. L., Li W.. Emergent and robust ferromagnetic-insulating state in highly strained ferroelastic LaCoO3 thin films. Nat. Commun. 2023;14:3638. doi: 10.1038/s41467-023-39369-6. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Chen S., Chang J. Y., Zhang Q., Li Q., Lin T., Meng F., Huang H., Si Y., Zeng S., Yin X., Duong M. N., Lu Y., Chen L., Guo E. J., Chen H., Chang C. F., Kuo C. Y., Chen Z.. Spin state disproportionation in insulating ferromagnetic LaCoO3 epitaxial thin films. Adv. Sci. 2023;10:2303630. doi: 10.1002/advs.202303630. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Huang T., Lyu Y., Huyan H., Ni J., Saremi S., Wang Y., Yan X., Yi D., He Q., Martin L. W., Xiang H., Pan X., Yu P.. Manipulation of the Ferromagnetism in LaCoO3 Thin Films Through Cation-Stoichiometric Engineering. Adv. Electron. Mater. 2023;9:2201245. doi: 10.1002/aelm.202201245. [DOI] [Google Scholar]
- Meng D., Guo H., Cui Z., Ma C., Zhao J., Lu J., Xu H., Wang Z., Hu X., Fu Z., Peng R., Guo J., Zhai X., Brown G. J., Knize R., Lu Y.. Strain-induced high-temperature perovskite ferromagnetic insulator. Proc. Nat. Acad. Sci. 2018;115:2873–2877. doi: 10.1073/pnas.1707817115. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Joshi T., Belanger D. P., Tan Y. T., Wen W., Lederman D.. Geometric influence on the net magnetic moment in LaCoO3 thin films. J. Mater. Res. 2023;38:2274–2286. doi: 10.1557/s43578-023-00957-3. [DOI] [Google Scholar]
- Mehta V. V., Liberati M., Wong F. J., Chopdekar R. V., Arenholz E., Suzuki Y.. Ferromagnetism in tetragonally distorted LaCoO3 thin films. J. Appl. Phys. 2009;105:07E503. doi: 10.1063/1.3059606. [DOI] [Google Scholar]
- Chaturvedi V., Walter J., Paul A., Grutter A., Kirby B., Jeong J. S., Zhou H., Zhang Z., Yu B., Greven M., Andre Mkhoyan K., Birol T., Leighton C.. Strain-induced majority carrier inversion in ferromagnetic epitaxial LaCoO3‑δ thin films. Phys. Rev. Mater. 2020;4:034403. doi: 10.1103/PhysRevMaterials.4.034403. [DOI] [Google Scholar]
- Zhang N., Tian X., Zhu Y., Wang Y., Tang Y., Zou M., Ma J., Feng Y., Geng W., Cao Y., Ma X.. Thickness Dependence of Oxygen Vacancy Ordering in Strained LaCoO3–x Thin Films. J. Phys. Chem. C. 2020;124:12492–12501. doi: 10.1021/acs.jpcc.0c02545. [DOI] [Google Scholar]
- Zhang N., Zhu Y., Li D., Pan D., Tang Y., Han M., Ma J., Wu B., Zhang Z., Ma X.. Oxygen Vacancy Ordering Modulation of Magnetic Anisotropy in Strained LaCoO3–x Thin Films. ACS Appl. Mater. Interfaces. 2018;10:38230–38238. doi: 10.1021/acsami.8b13674. [DOI] [PubMed] [Google Scholar]
- Lan Q. Q., Shen X., Yang H. W., Zhang H. R., Zhang J., Guan X. X., Yao Y., Wang Y. G., Yu R. C., Peng Y., Sun J. R.. Correlation between magnetism and “dark stripes” in strained La1–xSrxCoO3 epitaxial films (0 ≤ x ≤ 0.1) Appl. Phys. Lett. 2015;107:242404. doi: 10.1063/1.4937562. [DOI] [Google Scholar]
- Shin D., Yoon S., Song S., Park S., Lee H., Choi W.. Tunable Ferromagnetism in LaCoO3 Epitaxial Thin Films. Adv. Mater. Interfaces. 2022;9:2200433. doi: 10.1002/admi.202200433. [DOI] [Google Scholar]
- Guo E. J., Desautels R., Keavney D., Herklotz A., Ward T., Fitzsimmons M., Lee H.. Switchable orbital polarization and magnetization in strained LaCoO3 films. Phys. Rev. Mater. 2019;3:014407. doi: 10.1103/PhysRevMaterials.3.014407. [DOI] [Google Scholar]
- Guo E.-J., Desautels R., Keavney D., Roldan M. A., Kirby B. J., Lee D., Liao Z., Charlton T., Herklotz A., Ward T. Z., Fitzsimmons M. R., Lee H. N.. Nanoscale ferroelastic twins formed in strained LaCoO3 films. Science Adv. 2019;5:eaav5050. doi: 10.1126/sciadv.aav5050. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Yang F., Chris Hammel P.. FMR-driven spin pumping in Y3Fe5O12-based structures. J. Phys. D: Appl. Phys. 2018;51:253001. doi: 10.1088/1361-6463/aac249. [DOI] [Google Scholar]
- Kresse G., Furthmüller J.. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Phys. Rev. B. 1996;54:11169–11186. doi: 10.1103/PhysRevB.54.11169. [DOI] [PubMed] [Google Scholar]
- Kresse G., Furthmüller J.. Efficiency of ab-initio total energy calculations for metals and semiconductors using a plane-wave basis set. Comput. Mater. Sci. 1996;6:15–50. doi: 10.1016/0927-0256(96)00008-0. [DOI] [PubMed] [Google Scholar]
- Furness J. W., Kaplan A. D., Ning J., Perdew J. P., Sun J.. Accurate and Numerically Efficient r2SCAN Meta-Generalized Gradient Approximation. J. Phys. Chem. Lett. 2020;11:8208–8215. doi: 10.1021/acs.jpclett.0c02405. [DOI] [PubMed] [Google Scholar]
- Fuchs D., Dieterle L., Arac E., Eder R., Adelmann P., Eyert V., Kopp T., Schneider R., Gerthsen D., v. Löhneysen H.. Suppression of the ferromagnetic state in LaCoO3 films by rhombohedral distortion. Phys. Rev. B. 2009;79:024424. doi: 10.1103/PhysRevB.79.024424. [DOI] [Google Scholar]
- Fuchs D., Arac E., Pinta C., Schuppler S., Schneider R., v. Lohneysen H.. Tuning the magnetic properties of LaCoO3 thin films by epitaxial strain. Phys. Rev. B. 2008;77:014434. doi: 10.1103/PhysRevB.77.014434. [DOI] [Google Scholar]
- Shannon R. D.. Revised Effective Ionic Radii and Systematic Studies of Interatomic Distances in Halides and Chalcogenides. Acta Crystallogr., Sect. A. 1976;32:751–767. doi: 10.1107/S0567739476001551. [DOI] [Google Scholar]
- Glazer A. M.. The classification of tilted octahedra in perovskites. Acta Crystallogr. Sect. B. 1972;B28:3384–3392. doi: 10.1107/S0567740872007976. [DOI] [Google Scholar]
- Woodward P. M.. Octahedral tilting in perovskites I. Geometrical considerations. Acta Crystallogr. Sect. B. 1997;B53:32–43. doi: 10.1107/S0108768196010713. [DOI] [Google Scholar]
- Howard C. J., Stokes H. T.. Group theoretical analysis of octahedral tilting in perovskites. Acta Crystallogr. Sect. B. 1998;B54:782–789. doi: 10.1107/S0108768198004200. [DOI] [PubMed] [Google Scholar]
- Lufaso M. W., Woodward P. M.. Prediction of the crystal structures of perovskites using the software program SPuDS. Acta Crystallogr. Sect. B. 2001;57:725–738. doi: 10.1107/S0108768101015282. [DOI] [PubMed] [Google Scholar]
- Haas O., Struis R. P. W. J., McBreen J. M.. Synchrotron X-ray absorption of LaCoO3 perovskite. J. Solid State Chem. 2004;177:1000–1010. doi: 10.1016/j.jssc.2003.10.004. [DOI] [Google Scholar]
- Woodward D. I., Reaney I. M.. Electron diffraction of tilted perovskites. Acta Crystallogr. Sect. B. 2005;61:387–399. doi: 10.1107/S0108768105015521. [DOI] [PubMed] [Google Scholar]
- Lazić I., Bosch E. G. T., Lazar S.. Phase contrast STEM for thin samples: Integrated differential phase contrast. Ultramicroscopy. 2016;160:265–280. doi: 10.1016/j.ultramic.2015.10.011. [DOI] [PubMed] [Google Scholar]
- Groot F. de. Multiplet effects in X-ray spectroscopy. Coord. Chem. Rev. 2005;249:31–63. doi: 10.1016/j.ccr.2004.03.018. [DOI] [Google Scholar]
- Stavitski E., de Groot F. M. F.. The CTM4XAS program for EELS and XAS spectral shape analysis of transition metal L edges. Micron. 2010;41:687–694. doi: 10.1016/j.micron.2010.06.005. [DOI] [PubMed] [Google Scholar]
- Fujioka J., Yamasaki Y., Nakao H., Kumai R., Murakami Y., Nakamura M., Kawasaki M., Tokura Y.. Spin-Orbital Superstructure in Strained Ferrimagnetic Perovskite Cobalt Oxide. Phys. Rev. Lett. 2013;111:027206. doi: 10.1103/PhysRevLett.111.027206. [DOI] [PubMed] [Google Scholar]
- Viola M. C., Martínez-Lope M. J., Alonso J. A., Martínez J. L., De Paoli J. M., Pagola S., Pedregosa J. C., Fernández-Díaz M. T., Carbonio R. E.. Structure and magnetic properties of Sr2CoWO6: An ordered double perovskite containing Co2+(HS) with unquenched orbital magnetic moment. Chem. Mater. 2003;15:1655–1663. doi: 10.1021/cm0208455. [DOI] [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.