Robust Reconstruction of Atomic Force Microscopy Tip Shape From Force‐Indentation Curves

Logan J Kirsch 1, Jason P Killgore 2, Gregory J Rodin 3, Loukas F Kallivokas 4, Filippo Mangolini 1,5,✉
PMCID: PMC13745978  PMID: 42839695

ABSTRACT

A robust method, termed Piecewise Inverse Force Curve Analysis (PIFCA), is introduced for reconstructing the shape of atomic force microscopy (AFM) tips. The approach relies on piecewise linear axisymmetric approximation of the tip shape based on the analysis of force versus indentation depth curves acquired on a soft reference sample. PIFCA was validated using force curves collected on polydimethylsiloxane samples and was able to reconstruct nearly axisymmetric tip shapes with high goodness‐of‐fit (R 2 ≥ 0.98). PIFCA does not require any additional measurements such as electron microscopy or blind tip reconstruction (BTR). Thus, it simplifies the workflow and minimizes the risks of altering the tip shape and mechanical properties associated with those methods. Unlike other methods, PIFCA is robust for both deep and shallow indentations, which makes it particularly appealing for applications involving soft materials and deep indentations.

Keywords: contact mechanics, deep indentations of soft matter, nanomechanics, tip shape characterization


A robust method, termed Piecewise Inverse Force Curve Analysis (PIFCA), is introduced for reconstructing the shape of atomic force microscopy (AFM) tips. The approach relies on piecewise linear axisymmetric approximation of the tip shape based on the analysis of force versus indentation depth curves acquired on a soft reference sample.

graphic file with name SMTD-10-e71081-g006.webp

1. Introduction

Atomic force microscopy (AFM) has become a standard tool for measuring mechanical properties at the nanoscale. The simplest and most common method for performing such measurements is AFM force spectroscopy. In this technique, the AFM tip is indented into a sample (Figure 1). Following calibration of the cantilever spring constant and optical sensitivity of the AFM, one obtains an applied force P versus indentation depth δ curve, commonly referred to as a force curve. An appropriate contact mechanics model is then applied to the force curve data P(δ) to derive, most frequently, the composite elastic modulus E*. This quantity, defined as E∗=1−νs2/Es+1−νt2/Et−1, reflects the combined elastic response of the tip and the sample. Thus, for a tip with known Young's modulus Et and Poisson's ratio ν t , and an assumed sample Poisson's ratio ν s , the sample Young's modulus Es can then be calculated.

FIGURE 1.

FIGURE 1

Illustration of the AFM force spectroscopy process with example scanning electron microscopy (SEM) images for three types of AFM tips.

AFM force spectroscopy has attracted particular interest for characterizing soft biological [1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20] and polymer materials [21, 22, 23, 24, 25, 26, 27, 28, 29, 30]. These materials typically have Young's moduli less than 10 MPa [20, 31]. For example, AFM force curves have been acquired on cell structures to evaluate their nanoscale mechanical behavior [6, 8, 15, 20]. The results provided evidence that force curves can be used as a diagnostic tool to identify metastatic cancer cells [4, 7, 32]. However, the use of AFM force spectroscopy in clinical settings has been limited due to the challenges associated with performing quantitative E* measurements [4].

In AFM force spectroscopy, uncertainty about the tip shape has been repeatedly cited as one of the major sources of error [4, 9, 22, 27, 31, 33]. This uncertainty is detrimental for obtaining an accurate value of E* because its determination is strongly tip‐shape‐dependent [34]. The shape may vary significantly from tip to tip (Figure 1), and even within the same fabrication lot.

The shape of AFM tips is commonly determined using either electron microscopy or blind tip reconstruction (BTR). The advantages and disadvantages of these approaches have been discussed in the literature [27, 35, 36]. In summary, both approaches are intrusive, that is, they affect the shape and mechanical properties of the tip. In particular, electron microscopy measurements require moving the tip between the AFM and the electron microscope, which increases the risk of damaging the tip. Further, the presence of residual hydrocarbons in the electron microscope chamber may result in material deposition onto the tip, which can strongly affect both its shape and mechanical properties. Figure 2 shows three SEM images demonstrating the evolution of the same tip shape induced by material deposition during the imaging process.

FIGURE 2.

FIGURE 2

AFM tip shape evolution due to electron‐induced material deposition while acquiring electron microscopy images over the course of 1 min (acceleration voltage: 10 kV; emission current: 6 µA).

In BTR, the tip is used to image the topography of a hard reference sample with sharp features, which allows for reconstructing the tip shape [36, 37, 38]. A key advantage of this approach is that the reference sample is placed in the AFM, so the tip does not have to be moved for characterization to another instrument. However, BTR has two major drawbacks. First, probing hard reference samples can cause significant tip wear [39, 40]. Second, reference samples with topography capable of resolving the tip apex can only accurately reconstruct the first 20–50 nm of the tip height [24, 38, 39]. Knowledge of the tip shape over this spatial domain is often sufficient for nanomechanical measurements on hard materials because the indentation depths normally achieved are limited. However, it is insufficient for soft materials, for which indentation depths and contact areas are large. As a demonstration of the first point, Figure 3a displays SEM micrographs of a silicon AFM tip before and after scanning an ultrananocrystalline diamond (UNCD) surface, commonly used for BTR [41, 42, 43, 44], first in tapping mode and then in contact mode. The acquisition of topographic images to be used in BTR results in substantial tip blunting especially when imaging in contact mode. This is highlighted by the extracted tip profiles shown in Figure 3b (see SI8 for details on tip profile extraction from SEM images).

FIGURE 3.

FIGURE 3

(a) Superimposed and aligned SEM images of the same AFM tip (i) as‐received, (ii) after 1000 indentations on PDMS (with no perceptible changes from the as‐received condition), (iii) after a subsequent 500 × 500 nm tapping mode scan on UNCD (1.00 V free air amplitude, 0.65 V set point), and (iv) after a subsequent 500 × 500 nm contact mode scan on UNCD (10 nN setpoint); (b) Extracted tip profiles of the same AFM tip from the SEM images in (a). The profiles provide evidence of tip wear during BTR.

In addition to electron microscopy and BTR, several other techniques have been proposed for characterizing the AFM tip shape. In those methods, one does not fully reconstruct the shape but rather determines some of its parameters. For example, one can determine the radius of curvature at the tip apex from measurements of adhesion pull‐off forces [45, 46, 47, 48], cantilever beam dynamics [49, 50, 51], or indentations on reference samples with known mechanical properties [52, 53]. Such approaches can be used to identify parameters of canonical shapes such as cone, paraboloid, or power‐law near the tip apex. However, they require one to make a priori assumptions about the tip shape. In contrast, no such assumptions are required by electron microscopy and BTR. While such approximations are inherently restrictive, they may be sufficient for shallow indentations. In general, one may require more robust approximations, not restricted to canonical shapes, and capable of accurately describing the entire tip. Such approximations are critical for determining accurate E* from deep indentations.

In this work, we propose a tip shape characterization method that relies only on indenting a soft reference sample, with known E*, and does not require one to assume a canonical tip geometry. Thus, the proposed method does not require any measurements other than the force curves, and its accuracy is not limited to shallow indentations. This significantly simplifies the workflow and avoids difficulties associated with existing shape characterization methods.

2. Results and Discussion

In the proposed method, the tip shape is determined from the force curve data and known E*. Such problems are referred to as inverse, and they are ubiquitously sensitive to the input data and, in our case, the associated noise. This sensitivity is addressed by adopting well‐established filtering techniques. The proposed method does not involve any a priori assumptions based on canonical shapes. Rather, it relies on piecewise linear approximation, developed elsewhere [54, 55] for computing force curves for known tip shapes, that is, solving for E*. We refer to the proposed method as Piecewise Inverse Force Curve Analysis (PIFCA).

2.1. Background

The proposed method is based on Sneddon's relations [56] for axisymmetric contact between an indenter of arbitrary shape and an infinite elastic half‐space in the absence of friction or adhesion (Figure 4). Let the indenter shape be prescribed by an axisymmetric function h = f(r), where the cylindrical coordinates of a point on the indenter surface are (r, h). The height h is the distance from the tip apex along the symmetry axis of the indenter, and the radius r is the distance perpendicular to the symmetry axis. Sneddon's solution relates the indenter shape to the surface displacement field, giving P and δ in terms of E*, f(r), and the contact radius a: [56, 57, 58]

δ=∫0adfdraa2−r2dr (1)

and

P=2E∗∫0adfdrr2a2−r2dr (2)

FIGURE 4.

FIGURE 4

An axisymmetric indenter whose shape is described by the function f(r) pressed into an elastic half‐space with a force P, resulting in an indentation depth δ and contact radius a.

Thus, the forward problem is defined by Equations (1) and (2), which allow the calculation of the force P and the depth δ for a known f(r) and E* . Consequently, the continuous force curve P(δ) can also be parametrically defined in terms of the parameter a. In contrast, for the inverse problem at hand, f(r) is unknown, while E* is still treated as known. We suppose that the force curve data consists of pairs (Pm ,δ m ), where m = 0, 1, …N and the data have been preprocessed so that (P 0,δ0) = (0, 0). Here, we aim to compute a piecewise representation for f(r) based on (Pm ,δ m ) acquired on a system with a known E*.

2.2. PIFCA Method

During indentation, progressively larger sections of the AFM tip come into contact with the sample. Consequently, the associated force curve encodes information about progressively higher sections of the AFM tip shape with increasing indentation depths. The size of the encoded region for the tip is bounded by a. The PIFCA method is therefore based on two simple observations and one assumption. The first observation is that the initial radius of contact, corresponding to (P 0,δ0) = (0, 0), is a 0 = 0. The second observation is that as the indentation depth increases, f(r) for the portion of the tip in contact with the sample can be calculated from Sneddon's solution. The assumption is that f(r) can be accurately approximated by a piecewise linear function formed by N segments.

For the segment, 0 = a 0 ≤ r ≤ a 1, the unknown contact radius a 1 and segment slope k 1/2 are computed from Equations (1) and (2) using the pairs (P 0,δ0)and (P 1,δ1) (Figure 5a). This generates two equations, whose solution is the pair a 1 = P 1/(E*δ1) and k1/2=2E∗δ12/(πP1); this pair yields f(a 1) = k 1/2 a 1. Thus, both the lower bound a 1 and the function f(a 1) become available for the segment a 1 ≤ r ≤ a 2, and Equations (1) and (2) can be used to compute a 2 and k 3/2 and then the corresponding f(a 2) = f(a 1) + k 3/2(a 2 − a 1). Note that for the segment a 1 ≤ r ≤ a 2, it is natural to evaluate the integrals in Equations (1) and (2) over the segments [0, a 1] and [a 1,a 2]. In general, for a segment a m − 1 ≤ r ≤ am , the tip shape is then approximated as

fr=fam−1+km−1/2r−am−1. (3)

FIGURE 5.

FIGURE 5

PIFCA. (a) Physical basis for PIFCA. Increasing indentation leads to a growing contact radius a, so that successively larger portions of the AFM tip come in contact the sample. The tip shape f(r) is reconstructed piecewise, using the current force curve data point and the previously constructed segments, with each segment defined by its slope k. (b) The generalized process of the PIFCA method utilizing force curve data point (δ m ,Pm ) to reconstruct the tip node [am ,f(am )].

Once Equation (3) is substituted in Equation (1) and (2), one obtains: [54, 55]

δm=∫0amdhdramam2−r2dr=∑mi=1∫ai−1aidhdramam2−r2dr=am∑mi=1ki−1/2sin−1aiam−sin−1ai−1am (4)

and

Pm=2E∗∫0amdhdrr2am2−r2dr=2E∗∑mi=1∫ai−1aidhdrr2am2−r2dr=E∗∑i=1mki−1/2am2sin−1aiam−sin−1ai−1am−aiam2−ai2+ai−1am2−ai−12 (5)

Note that these are two equations with two unknowns, am and k m − 1/2, as ai and k i − 1/2 have been precomputed for all i < m. As Equations (4) and (5) are solved numerically for m = 1 to N, one obtains a fully reconstructed piecewise‐linear approximation for f(r) representing the AFM tip shape (Figure 5b).

2.3. Synthetic Data Analysis

As a demonstration, PIFCA is first applied to noise‐free and noisy synthetic force curve data. Also, this step is essential for identifying and addressing challenges associated with analyzing intrinsically noisy experimental data. All synthetic data considered here were generated using Equations. (1) and (2) applied to power‐law tips. This choice of f(r) = B 1 − n rn allows one to parameterize the shapes using lengths normalized by B, so that the shapes are defined by only one parameter (n). Figure 6a shows PIFCA being used to reconstruct the shapes for n = 1,   2, and 3, which represent well pristine AFM tips [59, 60, 61], for noise‐free data. In all cases, the coefficient of determination was R 2 = 1.00 for N = 100 force curve data points.

FIGURE 6.

FIGURE 6

Reconstruction of tip shape using PIFCA on synthetic force curves for power‐law (f(r) = B 1 − n rn ) indenters with differing values of n. Tip shape reconstruction using PIFCA on synthetic force curves without noise (a) and with noise (b); Tip reconstruction using PIFCA on noisy synthetic data after applying preprocessing steps and fitting a spline to the results of 10 force curves. The coordinates axes are normalized by B.

To process experimental force curves, PIFCA must also be able to handle data influenced by instrument noise. Figure 6b shows the results of applying PIFCA to the same synthetic data but randomized by adding Gaussian noise with zero mean and a standard deviation of 0.05 nN; a level typical for experimental force curves (SI2). The fits in Figure 6b are characterized by somewhat low values of R 2 ≤  0.90. For these noisy force curves, PIFCA consistently underpredicts the slope near the tip apex, where P and δ are small. Therefore, averaging the results from multiple force curves will not reduce the error.

To improve the fit accuracy, we apply three preprocessing steps (see SI3 for further details of the preprocessing steps and example MATLAB implementations):

  1. A forward and backward low‐pass de‐noising filter is applied to the force curve.

  2. The number of data points is down‐sampled to limit error accumulation over successive steps.

  3. The initial section of the force curve is rejected if it is still dominated by noise. To coarsely approximate this region, we assume a conical tip shape, and select the portion of the curve beginning at the first point beyond which the contact radius grows monotonically with δ. Notably, this contact radius can be calculated without assuming any parameters of the conical tip shape.

To further minimize the effects of noise, a cubic smoothing spline is fitted to the nodes found by performing PIFCA on multiple force curves (see SI4 for more details on the spline fitting steps).

Figure 6c shows the results of reconstructing f(r) using ten noisy synthetic force curves as the data. It is clear that the fitted nodes and the cubic splines provide excellent approximations (R 2 ≥ 0.99) to the synthetic f(r) profiles. The Supporting Information provides further information about error analysis regarding the fitting procedures, including the effects of preprocessing (Figure SI3), the number of force curves (Figure SI4), and the number of smoothing spline segments (Figure SI5).

2.4. Experimental Validation

Applying the PIFCA method requires an experimental setup consistent with the assumptions of the underlying Equations (1) and (2). That is, the experimental setup must minimize inelastic, finite‐size, and adhesion effects. Accordingly, the chosen experimental setup involves indentation of large (>1 mm in thickness) PDMS reference samples, which minimize inelasticity and size effects. Further, the indentations are performed in water after soaking the tip and sample in a surfactant solution to minimize adhesion. After indenting, the force curves were checked to ensure there was not a sudden decrease in force, which could be associated with piercing the PDMS sample [62]. This setup is discussed in more detail in Materials and Methods and evidence for the lack of adhesion and time dependence are presented in SI5 and SI6.

With this adopted setup, the PIFCA method was used to characterize three separate AFM tips whose SEM images, taken prior to indentation, are shown in Figure 7a. For the PDMS samples, E* = 2.23 ±   0.07 MPa (see details in Materials and Methods).

FIGURE 7.

FIGURE 7

The results of using PIFCA to experimentally characterize three AFM tips (a) SEM images of the three AFM tips. The third tip contains facets at higher sections causing significant deviations from axial symmetry; (b) Heat maps showing the distribution of 256 force curves acquired by indenting a PDMS reference sample with each tip; (c) Heat maps showing the distribution of the tip nodes predicted by performing PIFCA on the force curves; (d) Results after fitting a cubic smoothing spline to the tip nodes predicted by PIFCA; (e) Comparison of the fitted spline from PIFCA fits to the SEM tip profile. The shaded envelope displays the 95% confidence interval for the fitted spline.

Heatmaps of the 256 force curves obtained for each of the tips are shown in Figure 7b. Upon preprocessing, as described in the previous section and SI3, the data were used to generate the heatmaps of the tip nodes predicted by PIFCA (Figure 7c). Further, Figure 7d shows the results of fitting a cubic smoothing spline to these nodes as described in the previous section.

Figure 7e shows the comparison of the fitted spline (and its mirror about the center axis) to the SEM tip profile (extracted as described in SI8). Tips 1 and 2 both show excellent correlation to the SEM tip profile (R 2 ≥ 0.98). Tip 3 correlates well with the mean SEM tip profile near the apex (R 2 = 0.96 for height ≤ 30 nm) but fails to accurately capture the tip shape at higher sections. This inaccuracy is believed to be caused by significant deviations from axial symmetry, seen by the pyramidal facets in the corresponding SEM image for Tip 3. Further research is needed to quantify the errors in PIFCA associated with deviations from axial symmetry. Although the AFM cantilever is typically mounted at an angle relative to the sample surface (11° in our case), the resulting deviations from axial symmetry do not appear to be a major source of error based off the high correlation of the PIFCA results to the axisymmetric SEM profiles.

Figure 7e also shows a shaded envelope representing the 95% confidence interval for the fitted spline, obtained from Monte Carlo calculations [63]. These calculations account for variability between force curves and uncertainty in E*, cantilever spring constant, AFM optical sensitivity, and contact point (see SI9). Among the three tips, Tip 2 exhibits the largest uncertainty in the fitted spline, which is attributed to the lower nominal optical sensitivity in the associated measurements. Quantifying the overall uncertainty was sufficient for this work, but the individual uncertainty contributions could also be examined.

2.5. Additional Considerations

As stated in the introduction, common approaches for characterizing the tip geometry, that is, electron microscopy or BTR, may affect the shape and mechanical properties of the tips. To assess whether the acquisition of force curves on PDMS—a step required by the PIFCA method—induces variations in tip shape, SEM micrographs of a quartz AFM tip were collected before and after performing 1000 indentations on PDMS (Figure 3a). The extracted profiles, shown in Figure 3b, indicate no detectable changes in tip profile upon indenting PDMS. Note that using the same quartz AFM tip for subsequently scanning an UNCD surface to collect topographic images to be used in BTR [41, 42, 43, 44] results in substantial tip blunting, as discussed in the introduction. These results demonstrate that PIFCA significantly reduces the potential for tip wear by circumventing the need of either scanning hard specimens or employing tip characterization methods that may change the tip profile.

To minimize tip‐sample adhesion, indentations were performed in liquid after forming a surfactant passivation layer. Because this approach increases experimental complexity and contamination risk, we also evaluated PIFCA performance under adhesive conditions (i.e., in air and without any passivation layer) using synthetic and experimental data. Adhesive effects reduced the accuracy of PIFCA, but tip shape reconstructions approximately matching the SEM tip profile were still possible in air without a passivation layer (R 2 = 0.95 for the experimental force curves). Future research could further improve these approximations by incorporating adhesive effects into the PIFCA model. Conversely, to maximize accuracy while avoiding contamination, the AFM tip can be dried and UV‐ozone cleaned [64] after PIFCA. See SI10 for more details on the adhesion analysis.

For the highest measurement sensitivity, the reference sample should be selected such that the indentation stiffness approximately matches the AFM cantilever stiffness [65]. However, additional experiments using stiffer cantilevers (kc = 4.0 and 41.0 N/m) on the same PDMS reference sample still yielded PIFCA reconstructions highly correlated with the corresponding SEM tip profiles (R 2 ≥ 0.98). See SI11 for details on these experiments.

The failure to accurately reconstruct the non‐axisymmetric shape of Tip 3 indicates PIFCA cannot be used with non‐axisymmetric or broken AFM tips for general use. However, non‐axisymmetric indenter tips are often calibrated assuming an axisymmetric tip with an equivalent area‐to‐depth ratio [66]. Provided the tip model is sufficiently flexible to match this ratio, this calibration often introduces minimal error in force spectroscopy [67, 68]. Therefore, if the calibrated tip is being used for further force spectroscopy measurements, the PIFCA method will yield an equivalent axisymmetric tip profile that can be used for subsequent force spectroscopy analysis.

To compare the PIFCA method with techniques based on assumed canonical tip shapes, we analyzed the same force curve data from Figure 7b to calculate the tip radius Rt assuming a paraboloid tip shape, f(r) = r 2/2Rt (see SI12 for details). The paraboloid model was chosen for comparison because it is the most widely used in literature [2, 12, 15, 17, 19, 23, 28, 30, 31, 53, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79]. Figure 8 compares the resulting paraboloid tip shapes with the SEM tip profiles. For Tip 1, the correlation between the paraboloid and SEM tip profiles is only slightly worse than that obtained by PIFCA (R 2 = 0.97). However, this correlation begins to break down at higher sections of the tip (height >60 nm). For Tip 2, the paraboloid fit poorly correlates with the SEM tip profile (R 2 = 0.59). For Tip 3, both PIFCA and the paraboloid model correlate well with the SEM profile near the apex, but the paraboloid has stronger correlation at higher sections. However, the higher sections of Tip 3 are characterized by pyramidal facets such that no axisymmetric function can accurately describe the tip shape.

FIGURE 8.

FIGURE 8

Comparing the SEM tip profiles to profiles calculated by fitting the force curve data used for PIFCA assuming a paraboloid AFM tip shape.

3. Conclusions

In this work, we presented a method for reconstructing AFM tip shapes from force curve data. The method relies on piecewise linear approximations of the tip shape, with the presumption that the tip shape is axisymmetric. The mathematical foundation of the method is Sneddon's solution, so that the method is particularly well suited for stiff tips indenting soft samples with adhesion, inelastic, and size effects all minimized. The method was applied to both noise‐free and noisy synthetic data, which allowed us to identify additional necessary pre‐ and post‐processing steps. This enhanced version of the method was applied to force curve data acquired from an experimental setup specifically designed to meet the method's underlying assumptions. The experimental results further demonstrated the method accuracy, as long as the tips were close to being axisymmetric.

PIFCA overcomes two significant hurdles in the accurate characterization of AFM tip shape—a step required for high‐resolution quantitative AFM nanomechanical measurements. First, it circumvents the need for scanning hard samples, as required by BTR; this simplifies protocols and reduces the potential of AFM tip damage. This benefit is most pronounced when samples investigated following PIFCA do not cause significant tip wear. Second, it removes the requirement for lengthy ex‐situ electron microscopy to analyze the tip.

This work focused on applications to soft material nanomechanics, but PIFCA could be utilized in a number of other applications. For example, it could be used to nondestructively characterize tip wear when imaging hard samples. In addition, PIFCA could be applied to characterizing higher sections of AFM tips, which is required for accurate quantitative Kelvin Probe Force Microscopy [80].

Overall, PIFCA enables higher accuracy soft material nanomechanical measurements without the loss of lateral resolution due to tip wear. The linear‐piecewise nature of the fit offers greater flexibility in the fitted shape compared to canonical models. PIFCA serves as an excellent tool for accurate high‐throughput nondestructive AFM tip shape characterization.

4. Materials and Methods

4.1. Sample Preparation

The PDMS reference sample was prepared using a Dow SYLGARD 184 Silicone Elastomer Kit with a 5:1 base to curing agent ratio. After mixing and pouring into molds, the material was degassed and cured at 60°C for 12 h.

4.2. Surface Preparation

Before indenting, the PDMS reference sample and AFM cantilever were both soaked in a 2.8 wt. % commercial dish soap solution for ∼10 min, creating a passivation layer that minimizes adhesive interactions between the tip and sample [81].

4.3. E* Reference Value

Eref∗= 2.23 ±   0.07 MPa; Es = 1.67 ±  0.05 MPa measured via five ASTM D412‐A dumbbell uniaxial tension specimens cast from the same batch of PDMS and processed in parallel with the reference sample; ν s = 0.5 [82, 83, 84]; (1−νt2)/Et= 0.01 GPa−1 [33].

4.4. AFM Cantilevers

Tip 1: Bruker SAA‐HPI‐30, Spring constant kc = 0.182 N/m via laser doppler vibrometer [85]; Tip 2: NANOSENSORS qp‐BioAC, kc = 0.178 N/m via Sader method [86]; Tip 3: NANOSENSORS PPP‐CONTR, kc = 0.404 N/m via Sader method [86].

4.5. Experimental Force Curves

Tip 1: Asylum Cypher AFM, 256 indentations over a 5 x 5 µm lateral grid; Tip 2: Asylum MFP‐3D AFM, 256 indentations over a 5 x 5 µm lateral grid; Tip 3: Asylum Cypher AFM, 256 indentations over a 1 x 1 µm lateral grid. Force curves were performed in water to remove any adhesive effects from capillary condensation [87]. PIFCA was performed on the extension portion of all force curves.

Author Contributions

Logan J. Kirsch: conceptualization, investigation, writing – original draft, methodology, visualization, writing – review and editing, formal analysis, data curation. Jason P. Killgore: investigation, writing – review and editing, supervision, methodology. Gregory J. Rodin: writing – review and editing, writing – original draft, supervision, methodology. Loukas F. Kallivokas: methodology, writing – review and editing, supervision. Filippo Mangolini: supervision, funding acquisition, writing – review and editing, project administration, methodology.

Conflicts of Interest

The authors declare no conflicts of interest.

Supporting information

Supporting File: smtd71081‐sup‐0001‐SuppMat.docx.

SMTD-10-e71081-s001.docx (1.4MB, docx)

Acknowledgements

The material is based upon work supported by the National Science Foundation Faculty Early Career Development Program (Grant Number 2042304) and by the American Chemical Society Petroleum Research Fund (Grant Number 67062‐ND5).

Data Availability Statement

The data that support the findings of this study are available from the corresponding author upon reasonable request.

References

  • 1. Wu P.‐H., Aroush D. R.‐B., Asnacios A., et al., “A Comparison of Methods to Assess Cell Mechanical Properties,” Nature Methods 15 (2018): 491–498, 10.1038/s41592-018-0015-1. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 2. Krymskaya K. I., Andreeva N. V., and Filimonov A. V., “A Technique for Determining Young's Modulus of Biological Objects Using Atomic‐Force Microscopy in the Wide Temperature Range Below Rt,” Petersburg Polytechnical University Journal: Physics and Mathematics 2 (2016): 217. [Google Scholar]
  • 3. Rabe U., Atomic Force Acoustic Microscopy, in Applied Scanning Probe Methods II: Scanning Probe Microscopy Techniques, ed. Bhushan B. and Fuchs H. (Springer Berlin /Heidelberg, Berlin, Heidelberg, 2006): 37–90, 10.1007/3-540-27453-7_2. [DOI] [Google Scholar]
  • 4. Zemła J., Danilkiewicz J., Orzechowska B., Pabijan J., Seweryn S., and Lekka M., “Atomic Force Microscopy as a Tool for Assessing the Cellular Elasticity and Adhesiveness to Identify Cancer Cells and Tissues,” Seminars in cell & developmental biology 73 (2018): 115. [DOI] [PubMed] [Google Scholar]
  • 5. Lieber S. C., Atomic Force Microscopy Used to Determine the Young's Modulus of Vascular Smooth Muscle Cells (Master of Science, New Jersey Institute of Technology, 2002). [Google Scholar]
  • 6. Riedel R., Rani G., and Sengupta A., “Bacterial Adhesion on Soft Surfaces: The Dual Role of Substrate Stiffness and Bacterial Growth Stage,” Microorganisms 13 (2025): 637, 10.3390/microorganisms13030637. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 7. Lekka M., Gil D., Pogoda K., et al., “Cancer Cell Detection in Tissue Sections Using AFM,” Archives of Biochemistry and Biophysics 518 (2012): 151–156, 10.1016/j.abb.2011.12.013. [DOI] [PubMed] [Google Scholar]
  • 8. Viswanathan P., Ephstein Y., Garcia J. G. N., Cho M., and Dudek S. M., “Differential Elastic Responses to Barrier‐Altering Agonists in Two Types of Human Lung Endothelium,” Biochemical and Biophysical Research Communications 478 (2016): 599–605, 10.1016/j.bbrc.2016.07.112. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 9. Chang D., Hirate T., Uehara C., Maruyama H., Uozumi N., and Arai F., “Evaluating Young's Modulus of Single Yeast Cells Based on Compression Using an Atomic Force Microscope With a Flat Tip,” Microscopy and Microanalysis 27 (2021): 392. [DOI] [PubMed] [Google Scholar]
  • 10. Guz N., Dokukin M., Kalaparthi V., and Sokolov I., “If Cell Mechanics Can Be Described by Elastic Modulus: Study of Different Models and Probes Used in Indentation Experiments,” Biophysical Journal 107 (2014): 564–575, 10.1016/j.bpj.2014.06.033. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 11. Jaasma M. J., Jackson W. M., and Keaveny T. M., “Measurement and Characterization of Whole‐Cell Mechanical Behavior,” Annals of Biomedical Engineering 34 (2006): 748–758, 10.1007/s10439-006-9081-0. [DOI] [PubMed] [Google Scholar]
  • 12. Kurland N. E., Drira Z., and Yadavalli V. K., “Measurement of Nanomechanical Properties of Biomolecules Using Atomic Force Microscopy,” Micron 43 (2012): 116–128, 10.1016/j.micron.2011.07.017. [DOI] [PubMed] [Google Scholar]
  • 13. Villeneuve C., McCreery K. P., and Wickström S. A., “Measuring and Manipulating Mechanical Forces During Development,” Nature Cell Biology (2025): 575–590, 10.1038/s41556-025-01632-x. [DOI] [PubMed] [Google Scholar]
  • 14. Radmacher M., “Measuring the Elastic Properties of Biological Samples With the AFM,” IEEE Engineering in Medicine and Biology Magazine 16 (1997): 47–57, 10.1109/51.582176. [DOI] [PubMed] [Google Scholar]
  • 15. Wang X., Bleher R., Brown M. E., et al., “Nano‐Biomechanical Study of Spatio‐Temporal Cytoskeleton Rearrangements That Determine Subcellular Mechanical Properties and Endothelial Permeability,” Scientific Reports 5 (2015): 11097. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 16. Sirbuly D. J., Friddle R. W., Villanueva J., and Huang Q., “Nanomechanical Force Transducers for Biomolecular and Intracellular Measurements: Is There Room to Shrink and Why Do It?,” Reports on Progress in Physics 78 (2015): 024101, 10.1088/0034-4885/78/2/024101. [DOI] [PubMed] [Google Scholar]
  • 17. Encinar M., Casado S., Calzado‐Martín A., et al., “Nanomechanical Properties of Composite Protein Networks of Erythroid Membranes at Lipid Surfaces,” Colloids and Surfaces B: Biointerfaces 149 (2017): 174–183, 10.1016/j.colsurfb.2016.10.022. [DOI] [PubMed] [Google Scholar]
  • 18. White T., López‐Márquez A., Badosa C., et al., “Nanomechanics of Cell‐Derived Matrices as a Functional Read‐Out in Collagen VI‐Related Congenital Muscular Dystrophies,” Journal of The Royal Society Interface 22 (2025): 20240860, 10.1098/rsif.2024.0860. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 19. Guo S. and Akhremitchev B. B., “Packing Density and Structural Heterogeneity of Insulin Amyloid Fibrils Measured by AFM Nanoindentation,” Biomacromolecules 7 (2006): 1630–1636, 10.1021/bm0600724. [DOI] [PubMed] [Google Scholar]
  • 20. Vishnyakova P., Elchaninov A., Fatkhudinov T., and Kolesov D., “Unravelling Approaches to Study Macrophages: From Classical to Novel Biophysical Methodologies,” PeerJ 13 (2025): 19039, 10.7717/peerj.19039. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 21. Garcia R., “Nanomechanical Mapping of Soft Materials With the Atomic Force Microscope: Methods, Theory and Applications,” Chemical Society Reviews 49 (2020): 5850–5884, 10.1039/D0CS00318B. [DOI] [PubMed] [Google Scholar]
  • 22. VanLandingham M. R., Villarrubia J. S., Guthrie W. F., and Meyers G. F., “Nanoindentation of Polymers: An Overview,” Macromolecular Symposia 167 (2001): 15–44, 10.1002/1521-3900(200103)167:1<15::AID-MASY15>3.0.CO;2-T. [DOI] [Google Scholar]
  • 23. Dokukin M. E. and Sokolov I., “On the Measurements of Rigidity Modulus of Soft Materials in Nanoindentation Experiments at Small Depth,” Macromolecules 45 (2012): 4277–4288, 10.1021/ma202600b. [DOI] [Google Scholar]
  • 24. Clifford C. A. and Seah M. P., “Quantification Issues in the Identification of Nanoscale Regions of Homopolymers Using Modulus Measurement Via AFM Nanoindentation,” Applied Surface Science 252 (2005): 1915–1933, 10.1016/j.apsusc.2005.08.090. [DOI] [Google Scholar]
  • 25. Dokukin M. E. and Sokolov I., “Quantitative Mapping of the Elastic Modulus of Soft Materials With HarmoniX and PeakForce QNM AFM Modes,” Langmuir 28 (2012): 16060–16071, 10.1021/la302706b. [DOI] [PubMed] [Google Scholar]
  • 26. Kim S., Lee Y., Lee M., An S., and Cho S.‐J., “Quantitative Visualization of the Nanomechanical Young's Modulus of Soft Materials by Atomic Force Microscopy,” Nanomaterials 11 (2021): 1593. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 27. Yablon D. G., ed., Scanning Probe Microscopy in Industrial Applications: Nanomechanical Characterization (Wiley, 2014). [Google Scholar]
  • 28. Dimitriadis E. K., Horkay F., Maresca J., Kachar B., and Chadwick R. S., “Determination of Elastic Moduli of Thin Layers of Soft Material Using the Atomic Force Microscope,” Biophysical Journal 82 (2002): 2798–2810, 10.1016/S0006-3495(02)75620-8. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 29. Radmacher M., Fritz M., and Hansma P. K., “Imaging Soft Samples With the Atomic Force Microscope: Gelatin in Water and Propanol,” Biophysical Journal 69 (1995): 264–270, 10.1016/S0006-3495(95)79897-6. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 30. Simič R., Yetkin M., Zhang K., and Spencer N. D., “Importance of Hydration and Surface Structure for Friction of Acrylamide Hydrogels,” Tribology Letters 68 (2020): 64. [Google Scholar]
  • 31. Moeller G., “AFM Nanoindentation of Viscoelastic Materials With Large End‐Radius Probes,” Journal of Polymer Science Part B: Polymer Physics 47 (2009): 1573–1587, 10.1002/polb.21758. [DOI] [Google Scholar]
  • 32. Demichelis A., Divieto C., Mortati L., Pavarelli S., Sassi G., and Sassi M. P., “Toward the Realization of Reproducible Atomic Force Microscopy Measurements of Elastic Modulus in Biological Samples,” Journal of Biomechanics 48 (2015): 1099–1104, 10.1016/j.jbiomech.2015.01.023. [DOI] [PubMed] [Google Scholar]
  • 33. Hurley D. C., Contact Resonance Force Microscopy Techniques for Nanomechanical Measurements, in Appl. Scanning Probe Methods XI, ed. Bhushan B., and Fuchs H. (Springer Berlin /Heidelberg, Berlin, Heidelberg, 2009), 97–138, 10.1007/978-3-540-85037-3. [DOI] [Google Scholar]
  • 34. Wagner R., Moon R., Pratt J., Shaw G., and Raman A., “Uncertainty Quantification in Nanomechanical Measurements Using the Atomic Force Microscope,” Nanotechnology 22 (2011): 455703, 10.1088/0957-4484/22/45/455703. [DOI] [PubMed] [Google Scholar]
  • 35. Morozov I. A. and Izyumov R. I., “Challenges of Reliable AFM ‐Tip Shape Reconstruction and Approximation,” Microscopy Research and Technique 87 (2024): 105–113, 10.1002/jemt.24415. [DOI] [PubMed] [Google Scholar]
  • 36. Flater E. E., Zacharakis‐Jutz G. E., Dumba B. G., White I. A., and Clifford C. A., “Towards Easy and Reliable AFM Tip Shape Determination Using Blind Tip Reconstruction,” Ultramicroscopy 146 (2014): 130. [DOI] [PubMed] [Google Scholar]
  • 37. Villarrubia J. S., “Algorithms for Scanned Probe Microscope Image Simulation, Surface Reconstruction, and Tip Estimation,” Journal of Research of the National Institute of Standards and Technology 102 (1997): 425, 10.6028/jres.102.030. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 38. Dongmo L. S., Villarrubia J. S., Jones S. N., Renegar T. B., Postek M. T., and Song J. F., “Experimental Test of Blind Tip Reconstruction for Scanning Probe Microscopy,” Ultramicroscopy 85 (2000): 141–153, 10.1016/S0304-3991(00)00051-6. [DOI] [Google Scholar]
  • 39. Liu J., Notbohm J. K., Carpick R. W., and Turner K. T., “Method for Characterizing Nanoscale Wear of Atomic Force Microscope Tips,” ACS Nano 4 (2010): 3763–3772, 10.1021/nn100246g. [DOI] [PubMed] [Google Scholar]
  • 40. Vorselen D., Kooreman E. S., Wuite G. J. L., and Roos W. H., “Controlled Tip Wear on High Roughness Surfaces Yields Gradual Broadening and Rounding of Cantilever Tips,” Scientific Reports 6 (2016): 36972, 10.1038/srep36972. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 41. Vesicle Mechanics: A Push into the Nanoscale, PhD, Vrije Universiteit Amsterdam, 2016. [Google Scholar]
  • 42. Greiner C., Felts J. R., Dai Z., King W. P., and Carpick R. W., “Controlling Nanoscale Friction Through the Competition Between Capillary Adsorption and Thermally Activated Sliding,” ACS Nano 6 (2012): 4305–4313, 10.1021/nn300869w. [DOI] [PubMed] [Google Scholar]
  • 43. Cavallo F., Grierson D. S., Turner K. T., and Lagally M. G., ““Soft Si”: Effective Stiffness of Supported Crystalline Nanomembranes,” ACS Nano 5 (2011): 5400–5407, 10.1021/nn200461g. [DOI] [PubMed] [Google Scholar]
  • 44. Moldovan N., Dai Z., Zeng H., et al., “Advances in Manufacturing of Molded Tips for Scanning Probe Microscopy,” Journal of Microelectromechanical Systems 21 (2012): 431–442, 10.1109/JMEMS.2011.2174430. [DOI] [Google Scholar]
  • 45. Gotsmann B. and Lantz M. A., “Atomistic Wear in a Single Asperity Sliding Contact,” Physical Review Letters 101 (2008): 125501, 10.1103/PhysRevLett.101.125501. [DOI] [PubMed] [Google Scholar]
  • 46. Lantz M. A., Wiesmann D., and Gotsmann B., “Dynamic Superlubricity and the Elimination of Wear on the Nanoscale,” Nature Nanotechnology 4 (2009): 586–591, 10.1038/nnano.2009.199. [DOI] [PubMed] [Google Scholar]
  • 47. Bhaskaran H., Gotsmann B., Sebastian A., et al., “Ultralow Nanoscale Wear Through Atom‐by‐Atom Attrition in Silicon‐containing Diamond‐Like Carbon,” Nature Nanotechnology 5 (2010): 181–185, 10.1038/nnano.2010.3. [DOI] [PubMed] [Google Scholar]
  • 48. Lantz M. A., Gotsmann B., Jaroenapibal P., et al., “Wear‐Resistant Nanoscale Silicon Carbide Tips for Scanning Probe Applications,” Advanced Functional Materials 22 (2012): 1639–1645, 10.1002/adfm.201102383. [DOI] [Google Scholar]
  • 49. Killgore J. P., Geiss R. H., and Hurley D. C., “Continuous Measurement of Atomic Force Microscope Tip Wear by Contact Resonance Force Microscopy,” Small 7 (2011): 1018. [DOI] [PubMed] [Google Scholar]
  • 50. Santos S., Guang L., Souier T., Gadelrab K., Chiesa M., and Thomson N. H., “A Method to Provide Rapid in Situ Determination of Tip Radius in Dynamic Atomic Force Microscopy,” Review of Scientific Instruments 83 (2012): 043707, 10.1063/1.4704376. [DOI] [PubMed] [Google Scholar]
  • 51. Yamanaka K., Tsuji T., Noguchi A., Koike T., and Mihara T., “Nanoscale Elasticity Measurement With in Situ Tip Shape Estimation in Atomic Force Microscopy,” Review of Scientific Instruments 71 (2000): 2403–2408, 10.1063/1.1150627. [DOI] [Google Scholar]
  • 52. Borodich F. M. and Jin X., eds., Contact Problems for Soft, Biological and Bioinspired Materials (Springer; 2022). [Google Scholar]
  • 53. Monclus M. A., Young T. J., and Di Maio D., “AFM Indentation Method Used for Elastic Modulus Characterization of Interfaces and Thin Layers,” Journal of Materials Science 45 (2010): 3190–3197, 10.1007/s10853-010-4326-6. [DOI] [Google Scholar]
  • 54. Belikov S., Erina N., Huang L., et al., “Parametrization of Atomic Force Microscopy Tip Shape Models for Quantitative Nanomechanical Measurements,” Journal of Vacuum Science & Technology, B 27 (2009): 984. [Google Scholar]
  • 55. Belikov S., Magonov S., Erina N., et al., “Theoretical Modelling and Implementation of Elastic Modulus Measurement at the Nanoscale Using Atomic Force Microscope,” Journal of Physics: Conference Series 61 (2007): 1303–1307, 10.1088/1742-6596/61/1/257. [DOI] [Google Scholar]
  • 56. Sneddon I. N., “The Relation Between Load and Penetration in the Axisymmetric Boussinesq Problem for a Punch of Arbitrary Profile,” International Journal of Engineering Science 3 (1965): 47–57, 10.1016/0020-7225(65)90019-4. [DOI] [Google Scholar]
  • 57. Johnson K. L., Contact Mechanics (Cambridge Univ. Press, 1985), 10.1017/CBO9781139171731. [DOI] [Google Scholar]
  • 58. Barber J. R., Contact Mechanics (Springer International Publishing, 2018). [Google Scholar]
  • 59. Grierson D. S., Liu J., Carpick R. W., and Turner K. T., “Adhesion of Nanoscale Asperities With Power‐Law Profiles,” Journal of the Mechanics and Physics of Solids 61 (2013): 597–610, 10.1016/j.jmps.2012.09.003. [DOI] [Google Scholar]
  • 60. Carpick R. W., Agraït N., Ogletree D. F., and Salmeron M., “Measurement of Interfacial Shear (Friction) With an Ultrahigh Vacuum Atomic Force Microscope,” Journal of Vacuum Science & Technology, B 14 (1996): 1289. [Google Scholar]
  • 61. Kontomaris S. V., Malamou A., and Stylianou A., “The Hertzian Theory in AFM Nanoindentation Experiments Regarding Biological Samples: Overcoming Limitations in Data Processing,” Micron 155 (2022): 103228, 10.1016/j.micron.2022.103228. [DOI] [PubMed] [Google Scholar]
  • 62. Shrestha P., Geffner C., Jaffey M., et al., “Force Decomposition and Toughness Estimation From Puncture Experiments in Soft Solids,” Soft Matter 20 (2024): 5377–5388, 10.1039/D4SM00211C. [DOI] [PubMed] [Google Scholar]
  • 63. Coleman H. W., Experimentation, Validation, and Uncertainty Analysis for Engineers, Incorporated (John Wiley & Sons, 2018), 10.1002/9781119417989. [DOI] [Google Scholar]
  • 64. Thundat T., Zheng X.‐Y., Chen G. Y., Sharp S. L., Warmack R. J., and Schowalter L. J., “Characterization of Atomic Force Microscope Tips by Adhesion Force Measurements,” Applied Physics Letters 63 (1993): 2150–2152, 10.1063/1.110569. [DOI] [Google Scholar]
  • 65. Vanlandingham M. R., McKnight S. H., Palmese G. R., Eduljee R. F., Gillespie J. W., and McCulough J. R. L., “Relating Elastic Modulus to Indentation Response Using Atomic Force Microscopy,” Journal of Materials Science Letters 16 (1997): 117–119, 10.1023/A:1018533708655. [DOI] [Google Scholar]
  • 66. Pharr G. M., Oliver W. C., and Brotzen F. R., “On the Generality of the Relationship Among Contact Stiffness, Contact Area, and Elastic Modulus During Indentation,” Journal of Materials Research 7 (1992): 613–617, 10.1557/JMR.1992.0613. [DOI] [Google Scholar]
  • 67. King R. B., “Elastic Analysis of some Punch Problems for a Layered Medium,” International Journal of Solids and Structures 23 (1987): 1657–1664, 10.1016/0020-7683(87)90116-8. [DOI] [Google Scholar]
  • 68. Kirsch L. J., Killgore J. P., Rodin G. J., Weeks T. S., and Mangolini F., “Enhancing the Accuracy of Atomic Force Microscopy Measurements of Young's Modulus Via Force‐Curve‐Informed Tip Geometry Fitting,” Materials Today Nano 33 (2026): 100728, 10.1016/j.mtnano.2025.100728. [DOI] [Google Scholar]
  • 69. Shin H., Park J., Han S., Sastry A. M., and Lu W., “Component‐/Structure‐Dependent Elasticity of Solid Electrolyte Interphase Layer in Li‐Ion Batteries: Experimental and Computational Studies,” Journal of Power Sources 277 (2015): 169–179, 10.1016/j.jpowsour.2014.11.120. [DOI] [Google Scholar]
  • 70. Zhang T., Ma L., Ling S., et al., “Protocol for Measuring the Young's Modulus of Organoids Using Atomic Force Microscopy,” STAR Protocols 6 (2025): 103825, 10.1016/j.xpro.2025.103825. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 71. Guo Y., Lin Y.‐T., Choi J., et al., “Surface Chemistry of an Acrylosilane‐Melamine Based Automotive Clearcoat,” Industrial & Engineering Chemistry Research 64 (2025): 5982–5994, 10.1021/acs.iecr.4c04162. [DOI] [Google Scholar]
  • 72. Saad Ejweada Bodowara F., Determination of Local Elastic Modulus of Soft Biomaterial Samples Using AFM, Doctor of Philosophy in Chemistry (Florida Institute of Technology, 2018). [Google Scholar]
  • 73. Heuberger M., Dietler G., and Schlapbach L., “Mapping the Local Young's Modulus by Analysis of the Elastic Deformations Occurring in Atomic Force Microscopy,” Nanotechnology 6 (1995): 12–23, 10.1088/0957-4484/6/1/003. [DOI] [Google Scholar]
  • 74. Cheng Q., Ye D., Yang W., et al., “Construction of Transparent Cellulose‐Based Nanocomposite Papers and Potential Application in Flexible Solar Cells,” ACS Sustainable Chemistry & Engineering 6 (2018): 8040–8047, 10.1021/acssuschemeng.8b01599. [DOI] [Google Scholar]
  • 75. Zhang Z., Said S., Smith K., et al., “Characterizing Batteries by In Situ Electrochemical Atomic Force Microscopy: A Critical Review,” Advanced Energy Materials 11 (2021): 2101518. [Google Scholar]
  • 76. Roa J. J., Oncins G., Diaz J., Sanz F., and Segarra M., “Calculation of Young's Modulus Value by Means of AFM,” Recent Patents on Nanotechnology 5 (2011): 27. [DOI] [PubMed] [Google Scholar]
  • 77. Liu Y., Sokolov I., Dokukin M. E., Xiong Y., and Peng P., “Can AFM Be Used to Measure Absolute Values of Young's Modulus of Nanocomposite Materials Down to the Nanoscale?,” Nanoscale 12 (2020): 12432–12443, 10.1039/D0NR02314K. [DOI] [PubMed] [Google Scholar]
  • 78. Zhou Y., Kastner M. J., Tighe T. B., and Du J., “Elastic Modulus Mapping for Bovine Cortical Bone From Submillimeter‐ to Submicron‐Scales Using PeakForce Tapping Atomic Force Microscopy,” Extreme Mechanics Letters 41 (2020): 101031, 10.1016/j.eml.2020.101031. [DOI] [Google Scholar]
  • 79. Soofi S. S., Last J. A., Liliensiek S. J., Nealey P. F., and Murphy C. J., “The Elastic Modulus of Matrigel™ as Determined by Atomic Force Microscopy,” Journal of Structural Biology 167 (2009): 216–219, 10.1016/j.jsb.2009.05.005. [DOI] [PMC free article] [PubMed] [Google Scholar]
  • 80. Zahmatkeshsaredorahi A., Millan‐Solsona R., Jakob D. S., Collins L., and Xu X. G., “Kelvin Probe Force Microscopy Under Ambient Conditions,” Nature Reviews Methods Primers 5 (2025): 53, 10.1038/s43586-025-00424-9. [DOI] [Google Scholar]
  • 81. Ebenstein D. M., “Nano‐JKR Force Curve Method Overcomes Challenges of Surface Detection and Adhesion for Nanoindentation of a Compliant Polymer in Air and Water,” Journal of Materials Research 26 (2011): 1026–1035, 10.1557/jmr.2011.42. [DOI] [Google Scholar]
  • 82. Müller A., Wapler M. C., and Wallrabe U., “A Quick and Accurate Method to Determine the Poisson's Ratio and the Coefficient of Thermal Expansion of PDMS,” Soft Matter 15 (2019): 779. [DOI] [PubMed] [Google Scholar]
  • 83. Seghir R. and Arscott S., “Extended PDMS Stiffness Range for Flexible Systems,” Sensors and Actuators A: Physical 230 (2015): 33–39, 10.1016/j.sna.2015.04.011. [DOI] [Google Scholar]
  • 84. Mark J., Polymer Data Handbook (Oxford University Press, 1999). [Google Scholar]
  • 85. Ohler B., “Cantilever Spring Constant Calibration Using Laser Doppler Vibrometry,” Review of Scientific Instruments 78 (2007): 063701, 10.1063/1.2743272. [DOI] [PubMed] [Google Scholar]
  • 86. Sader J. E., Chon J. W. M., and Mulvaney P., “Calibration of Rectangular Atomic Force Microscope Cantilevers,” Review of Scientific Instruments 70 (1999): 3967–3969, 10.1063/1.1150021. [DOI] [Google Scholar]
  • 87. Mate C. M. and Carpick R. W., Tribology on the Small Scale: A Modern Textbook on Friction, Lubrication, and Wear (Oxford University PressOxford, 2019), 10.1093/oso/9780199609802.001.0001. [DOI] [Google Scholar]

Associated Data

This section collects any data citations, data availability statements, or supplementary materials included in this article.

Supplementary Materials

Supporting File: smtd71081‐sup‐0001‐SuppMat.docx.

SMTD-10-e71081-s001.docx (1.4MB, docx)

Data Availability Statement

The data that support the findings of this study are available from the corresponding author upon reasonable request.


Articles from Small Methods are provided here courtesy of Wiley

RESOURCES