Abstract
Biomass-derived pomegranate peel carbon dots (PP-CDs) were incorporated into sol–gel silica coatings to develop environmentally sustainable protective films for stainless steel 304 in hydrochloric acid and the effect of PP-CDs loading on coating microstructure and corrosion resistance was investigated. The PP-CDs were prepared hydrothermally and characterized by TEM, FT-IR XPS, UV-vis and photoluminescence spectroscopy. They are spherical, photoluminescent particles (average diameter ∼ 7.4 nm) with hydroxyl, carbonyl and carboxyl surface groups. To examine their fate during processing, the SiO2-0.003PP-CD material was also studied as a calcined powder (500 °C, 2 h) by TEM and XPS, which showed nanoscale features of about 3.0 nm without noticeable aggregation, the presence of C, N, O and Si, and a shift of the O 1s peaks to lower binding energy relative to pristine PP-CDs. SiO2 coatings containing 0, 0.003 and 0.005 mg PP-CDs were deposited on S304 by spin-coating and calcined at 500 °C. Their microstructure, composition and wettability were examined by SEM, EDS and contact angle measurements and their corrosion behavior after 24 h in 1 M HCl at 25 °C by EFM, PDP and EIS. Among the investigated compositions, the SiO2-0.003PP-CDs coating exhibited the most continuous microstructure, maintaining its integrity after immersion in 1.0 M HCl, whereas the undoped coating underwent severe cracking and delamination. Electrochemical measurements (EFM, PDP, and EIS) gave the same ranking, with inhibition efficiencies of 84–86% (EFM and PDP) for the 0.003 mg coating compared with 50–53% for undoped silica. EDS, contact angle, and AFM results were consistent with better retention of the 0.003 mg coating after immersion. The improvement over the undoped coating is primarily attributed to the addition of PP-CDs, which is accompanied by a change in film morphology and microstructure, from a cracked, agglomerated film to a continuous, more homogeneous one at 0.003 mg. These findings indicate that biomass-derived carbon dots can improve the short-term corrosion resistance of sol–gel silica coatings on stainless steel in hydrochloric acid under laboratory conditions.
Pomegranate peel-derived carbon dots gave a continuous sol–gel silica coating on 304 stainless steel in place of a cracked one, raising inhibition efficiency in 1.0 M HCl from about 50% to about 85% in short-term laboratory tests.
1. Introduction
Among the various stainless steel grades, 304 stainless steel (S304) is one of the most widely used owing to its excellent combination of mechanical strength, formability, weldability, and corrosion resistance. Consequently, it has found extensive applications in aerospace, petrochemical, chemical processing, food processing, and biomedical industries. Its corrosion resistance primarily arises from the spontaneous formation of a thin, adherent, and self-healing chromium-rich passive oxide film on the surface, which effectively isolates the underlying metal from many corrosive environments.1,2 However, this passive layer can become unstable under aggressive conditions, particularly in acidic media containing high concentrations of chloride ions, leading to localized corrosion, passive film breakdown, and premature failure of engineering components.2 Therefore, the development of efficient and environmentally sustainable surface protection strategies remains a critical challenge for extending the service life of stainless steel materials.
Ceramic coatings have been widely investigated as protective barriers for stainless steel and other metallic substrates owing to their chemical stability. Single-oxide coatings based on SiO2,3,4 TiO2,5,6 Al2O3,7,8 ZrO2,8,9 CeO2 10,11 and HfO2,12,13 as well as mixed-oxide systems such as SiO2–TiO2,14 ZrO2–TiO2,15 SiO2–ZrO2,16,17 TiO2–CeO2,18,19 ZrO2–CeO2,20,21 and Eu:Y2Ti2O7 22 have shown notable protection in chloride-containing and acidic environments.
Among the deposition routes, the sol–gel process is particularly attractive because of its low processing temperature, ease of handling, control over molecular structure, and ability to coat complex shapes.23 Within this field, sol–gel SiO2 is the most widely used matrix for corrosion protection of metals due to low cost, chemically inert, good adhesiveness to the substrate and stable in acidic and chloride media.3,23,24 On stainless steel, thin silica films have been shown to lower corrosion current densities markedly in acidic and chloride media.25
Despite these advantages, the protective performance of conventional sol–gel SiO2 is limited by its microstructure. Sol–gel silica is intrinsically mesoporous, and the nanometric to submicron thickness of typical films is frequently insufficient to provide the barrier capacity required for long-term protection.24 Moreover, the high residual stress generated during drying and thermal curing makes these coatings susceptible to microcracking, which further increases their porosity and reduces their corrosion resistance.24,26,27 The resulting pores and microcracks form continuous pathways through which the electrolyte can diffuse to the coating/substrate interface and initiate corrosion of the underlying metal.3,28 Conventional SiO2 coatings therefore face a trade-off between thin, crack-free films with limited barrier performance and thicker films that are more prone to stress-induced failure.23,29
Several strategies have been proposed to address this trade-off. Multilayer deposition increases thickness and improves protection, and loading the sol–gel matrix with corrosion inhibitors, including through nanocontainers, adds active protection.23 Hybrid organic–inorganic coatings combine the barrier properties of ceramic oxides with improved flexibility, adhesion, and mechanical stability, which helps overcome the brittleness and defect formation of purely inorganic coatings,22,27 and their higher solid content reduces shrinkage and residual stress.29 Examples include SiO2/ZrO2 hybrid layers doped with corrosion inhibitor nanoparticles, which form an insoluble interface between the substrate and a gradient coating and provide self-protecting capacity,30 and biochar- and zeolite-based carbon/silica coatings for 7075 aluminum alloy.31 Surface-treated silica nanoparticles have also improved homogeneity and suppressed crack propagation in a sol–gel coating on mild steel.26 However, these approaches generally add processing steps or formulation components, such as multilayer deposition, inhibitor loading, or surface-treated fillers,23,26 and the way the additive influences silica hydrolysis and condensation is rarely the focus of these studies. A simple, sustainable additive that helps regulate network formation without extra processing steps is therefore of interest.
Carbon dots (CDs) are zero-dimensional, chemically stable and biocompatible nanoparticles whose surfaces carry abundant hydroxyl and carboxyl groups that can interact with hydrolyzed silanol species and integrate into the inorganic network.29,32–34 Consistent with this, adding 50 ppm carbon quantum dots to a sol–gel silica coating on AM60B magnesium alloy eliminated micrometric cracks through chemical bonding with the silica network, and the resulting reduction in electrolyte penetration was attributed to pore blocking and the absence of these cracks.35 Biomass-derived carbon quantum dots likewise reduced connected pore pathways and formed a uniform layer that limited electrolyte penetration in a coating on steel.36 CDs may therefore address the limitations described above in two ways. Their nanoscale size may allow them to fill pores and lengthen the electrolyte pathway,37 and their surface groups may moderate silica hydrolysis and condensation, promoting a more uniform network with fewer shrinkage-related cracks and defects.33–35,38 These roles are proposed in the literature and have been tested in only a few systems.
Biomass is an attractive CD precursor owing to its abundance, low cost, sustainability, and oxygen-rich surface chemistry,31 and biomass-derived CDs have been applied in surface engineering,39,40 wettability modulation,41,42 self-cleaning coatings,34 anticounterfeiting,43,44 latent fingerprint visualization,45,46 chemical sensing,47,48 bioimaging,49–51 and environmental remediation,52,53 with emerging use as nanomodifiers in coating systems.27 Pomegranate peel is an abundant fruit-processing waste rich in polyphenols such as ellagic acid, tannins, and flavonoids, and CDs prepared from it retain hydroxyl, carboxyl, and carbonyl surface groups derived from these compounds.54
Carbon dots have been explored in sol–gel coatings on only a few substrates,35,36 and, to the best of our knowledge, pomegranate peel-derived CDs have not been used as nanostructure-directing additives in sol–gel SiO2 coatings for stainless steel. How such CDs influence silica network formation, coating compactness, and short-term protection in acidic chloride media has received very little attention, and the dependence on loading is unclear.
The objectives of this work were therefore to (i) incorporation pomegranate peel-derived CDs (PP-CDs), a waste-derived additive into a sol–gel silica coating on 304 stainless steel (S304); (ii) characterize PP-CDs and their state after calcination in the silica matrix, (ii) examine how PP-CD loading affects coating morphology, wettability and stability after immersion in 1.0 M HCl, and (iii) evaluate the corrosion behavior of the coatings on S304 by EFM, PDP and EIS. The study is relevant scientifically because it examines how a biomass-derived nanoadditive is associated with changes in a sol–gel silica film, and technologically because it explores a low-cost, waste-derived route to protecting stainless steel in hydrochloric acid. The coatings were evaluated on laboratory 304 stainless steel coupons after 24 h at 25 °C in strongly acidic, chloride-containing medium. Hydrochloric acid is widely used for acid cleaning, pickling, descaling and oil-well acidizing55,56 and 1.0 M HCl is commonly used to mimic industrial acid-cleaning conditions for stainless steel.57 In such media, the combined action of H+ and Cl− destabilizes the chromium-rich passive film and promotes active dissolution and localized corrosion.56 This is a short-term laboratory study and does not aim to establish long-term performance or the detailed mechanism.
2. Experimental
2.1. Materials
Fresh pomegranate peels were collected and used as the carbon precursor for the synthesis of carbon dots. Tetraethyl orthosilicate (TEOS) were obtained from Aldrich and used as received without further purification. Absolute ethanol, acetone and hydrochloric acid (HCl) were obtained from BDH. Distilled water was used throughout all experiments. Dialysis bags with molecular weight cutoff equal 1 kD (1 kD MWCO) was purchased from Frey Scientific Company.
2.2. Instruments and measurement
The morphology of the PP-CDs and of the calcined SiO2-0.003PP-CDs nanopowder was examined by transmission electron microscopy (TEM) on a JEOL JEM-2100CX microscope. The nanopowder was prepared by the same sol–gel procedure as the coatings, dried at 80 °C and calcined at 500 °C for 2 h. Particle sizes were measured directly on the micrographs and are reported as approximate mean values. UV-vis spectra of the PP-CDs were recorded using a JASCO V-530 spectrophotometer (Japan). Photoluminescence (PL) emission was measured using a PerkinElmer LS55 luminescence spectrometer (USA). FT-IR spectra were recorded in the range of 4000–400 cm−1 by a Nicolet 6700 FT-IR spectrometer using KBr discs. X-ray photoelectron spectroscopy (XPS) was performed on an AXIS Nova spectrometer with monochromatized Al Kα radiation to analyze the surface elements and chemical states of the pristine PP-CDs and of the calcined SiO2-0.003PP-CDs nanopowder, and high-resolution spectra (C 1s, O 1s, N 1s and Si 2p) were fitted to obtain the components reported in Section 3.1.
X-ray diffraction patterns of coated samples were recorded using a (Bruker D8 Advance X-ray diffractometer, Cu Kα radiation (λ = 1.5406 Å)). The surface topography was investigated using atomic force microscopy (AFM) technique with a Nano surf C3000 instrument (Nano surf AG, Graubernstr 12, CH-4410 Liestal – Switzerland). The images were acquired in phase contrast mode using NCLR cantilever type with a spring constant of 0.15 N m−1 at a resonance frequency of 13 kHz. All images were recorded under ambient air conditions at room temperature (25 °C ± 1). The surface morphology of thin films was examined using high-resolution scanning electron microscopy (SEM) with an energy dispersive spectroscopic (EDS) microanalysis system. The SEM analysis was performed using a Quanta FEG 250 instrument with a field emission gun from FEI Company in the Netherlands at an accelerating voltage of 30 kV, a spot size of 3.5 and working distances of 10.8–15.3 mm. Images were acquired with an Everhart–Thornley detector (ETD) in secondary-electron mode. Magnifications ranged from 60 000× to 100 000× (horizontal field width 4.14–6.91 µm), and the magnification, detector and scale bar are given in the data bar of each micrograph. EDS spectra were acquired at an accelerating voltage of 30 kV and a magnification of 500× from area scans over the full field of view (image resolution 512 × 442 pixels, pixel size 1.50 µm, corresponding to an analysed area of approximately 0.77 × 0.66 mm). Prior to SEM imaging and EDS analysis, the thin films were coated with a thin layer of gold by sputtering to prevent surface charging. The micrographs shown are images from selected regions of each specimen, and the observations are therefore treated as qualitative. In contact angle method, water droplets were deposited on the surfaces of the thin films. The contact angle measurements were performed using a Shape Analysis System model DSA258 instrument from KRUSS GmbH. The drop images were captured over time using a video camera, and an image analysis was conducted to determine the contact angle.
2.3. Preparation methods
2.3.1. Preparation of PP-CDs
Carbon dots (PP-CDs) were synthesized from pomegranate peel extract using a hydrothermal method. Fresh pomegranate peels were thoroughly washed with distilled water to remove dust and impurities and then cut into small pieces. The peel pieces were transferred to a flask containing distilled water and heated on a hot plate for approximately 30 min to obtain the extract. After cooling to room temperature, the extract was filtered to remove solid residues. The obtained pomegranate peel extract was then transferred into a Teflon-lined stainless-steel autoclave and heated at 200 °C for 48 h. After the hydrothermal reaction, the autoclave was allowed to cool naturally to room temperature. The resulting carbon dot suspension was centrifuged for 10 min to remove large particles and insoluble residues. The supernatant containing the carbon dots was further purified by dialysis using a dialysis membrane (MWCO = 1000 Da) to remove small molecular impurities and unreacted species. Finally, the purified carbon dot solution was freeze-dried to obtain PP-CDs as a brown powder.
2.3.2. Preparation of PP-CDs/SiO2 precursor solution
SiO2-PP-CDs nanocomposites were prepared by a sol–gel method. A PP-CDs stock dispersion was prepared by dispersing 0.002 g of PP-CDs, weighed on an analytical balance (readability [0.1 mg]), in 1000 mL of distilled water, giving a concentration of 0.002 mg mL−1. For the PP-CD-containing sols, 1.5 or 2.5 mL of this stock (0.003 mg or 0.005 mg of PP-CDs, respectively) was used as part of the 5 mL aqueous phase and made up to 5 mL with distilled water. This aqueous phase was mixed with 20 mL of absolute ethanol and three drops of HCl and stirred for 20 min. Then 2 mL of TEOS was added dropwise and the mixture was stirred for 30 min to promote hydrolysis and initiate condensation, followed by continuous stirring for 3 h to ensure homogeneous dispersion of the PP-CDs. The final sols (about 27 mL) contained 0.003 mg and 0.005 mg of PP-CDs. A PP-CD-free SiO2 sol, prepared with 5 mL of distilled water, served as the reference. The PP-CD concentrations were selected to systematically evaluate the effect of carbon-dot loading on the microstructure, surface properties, and corrosion-protection performance of the sol–gel derived SiO2 coatings and to identify the concentration providing the most favorable overall coating performance. For TEM and XPS analyses, the SiO2-0.003PP-CDs nanopowder was prepared using the same procedure described above, followed by drying at 80 °C and calcination at 500 °C for 2 h.
2.3.3. Preparation of PP-CDs/SiO2 coated stainless steel
Austenitic stainless steel plates (304) with dimensions of 2 cm × 1 cm × 0.1 mm were employed as the substrates. Prior to the application of the coating, the substrates underwent a series of mechanical polishing steps utilizing SiC abrasive papers of various grit sizes, namely 320, 400, 600, 800, 1200, 1500, and 2000. Afterward, the substrates were subjected to ultrasonic cleaning for 10 minutes each, using acetone, ethanol, and distilled water, respectively, and followed by thorough drying. The undoped and PP-CDs doped SiO2 film were prepared by immediately spin-coated of previously prepared silica precursor solution onto the surface-prepared stainless steel 304 substrates at 3000 rpm for 1 minute. The coated substrates were dried at 80 °C for 45 minutes and then calcinated at 500 °C for 2 hours. The prepared samples are denoted by S304-SiO2, S304-SiO2-0.003PP-CDs, and S304-SiO2-0.005PP-CDs.
2.4. Electrochemical quantification of S304 corrosion in acidic media
Electrochemical testing was performed at 25 °C using a standard three-electrode configuration: a 304 stainless steel coupons with dimensions of 2 cm × 1 cm × 0.1 mm were carefully used and as working electrode (stabilized for 60 min at Open Circuit Potential, OCP). S304 have the following composition (1.1%C, 1.2%O, 0.9%Al, 18.8%Cr, 7.3%Ni and the remained is Fe, 70.8%). The exposed surface was mechanically abraded and polished with emery papers up to 4/0 grit size. These polished samples cleaned with acetone, washed with double-distilled water and finally dried at room temperature.
A platinum-mesh counter electrode isolated behind fritted glass, and an SCE reference coupled through a Luggin capillary to reduce IR drop. The corrosive medium, 1.0 M HCl, was prepared by diluting analytical grade 37% hydrochloric acid with double distilled water. S304 corrosion in 1.0 M HCl was evaluated with and without studied compounds by EIS, PDP, and EFM. All of the electrochemical experiments were performed under stirring. Experiments were conducted on a Gamry 3000 Potentiostat/Galvanostat/ZRA running Gamry Framework (ESA400), with analysis in Echem Analyst 6.33 (modules: dc105, EIS300, EFM140). Polarization scans were collected from −1000 to +1000 mV relative to OCP at 0.005 V s−1. Impedance spectra were recorded using a 10 mV (peak-to-peak) perturbation from 100 kHz down to 20 mHz. EFM was executed with dual perturbations at 2.0 and 5.0 Hz (base 1.0 Hz), each at 10 mV amplitude. All electrochemical measurements were performed in triplicate, (n = 3), using independently prepared specimens under identical experimental conditions to ensure the reproducibility and reliability of the experimental results.
The reported values represent the mean of three independent measurements and are expressed as mean ± standard deviation (SD). The standard deviation was calculated to evaluate the variability and reproducibility of the experimental measurements. Where applicable, the corresponding SD values are presented as error bars in the relevant figures.
3. Results and discussion
3.1. Characterization of PP-CDs and SiO2-0.003 PP nanopowder
TEM was used to examine the morphology and size of the PP-CDs. The particles are spherical (Fig. 1a), with an average diameter of ∼7.4 nm. The FT-IR spectrum of the hydrothermally prepared PP-CDs (200 °C, 48 h) shows a broad O–H/N–H stretching band at ∼3200–3500 cm−1, weak sp3 C–H bands at ∼2850–2950 cm−1, and a strong band at ∼1650 cm−1 from C O/C C stretching of conjugated carbonyl or aromatic groups (Fig. 1b). Bands at ∼1350–1400 cm−1 (C–N stretching, O–H bending) and ∼1050–1100 cm−1 (C–O–C stretching) are also present, and weak bands at 600–900 cm−1 (aromatic C–H bending) are consistent with a partially graphitized aromatic core58 The UV-vis spectrum of the PP-CDs shows an absorption peak at 230 nm and a tail from about 270 to 400 nm (Fig. 1c), assigned to π → π* transitions of the C C bonds in the graphitic core and n → π* transitions of surface groups such as C O.58 The PP-CDs show a broad emission band centered at about 440 nm (λex = 360 nm; Fig. 1d). This broadening is consistent with the structural heterogeneity of carbon dots, in particular the variety of surface groups.58
Fig. 1. TEM, HR-TEM images (a); FT-IR (b); absorption (c) and emission spectra (d) of PP-CDs nanopowder prepared by hydrothermal method for 48 h at 200 °C.

XPS was used to examine the elemental composition and surface groups of the PP-CDs. The survey spectrum shows carbon, nitrogen, and oxygen (Fig. 2). The C 1s spectrum resolves into three components at 284.82, 286.21, and 288.69 eV, assigned to C–C/C C, C–N/C–O, and O–C O, and the dominant C–C/C C component suggests partial graphitization during hydrothermal synthesis. The O 1s spectrum shows C O, C–OH, and C–O–C contributions (532.58, 533.25, and 534.44 eV), and the N 1s spectrum two components at 401.00 and 402.78 eV, assigned to graphitic and amino-type nitrogen, indicating nitrogen doping of the carbon core.58 Together, these results indicate hydroxyl, carbonyl, and carboxyl groups on the PP-CD surface.
Fig. 2. (a) Full scan XPS, high resolution spectra of (b) C 1s (c) O 1s and (d) N 1s of PP-CDs nanopowder prepared by hydrothermal method for 48 h at 200 °C.

To investigate whether pomegranate peel-derived carbon dots (PP-CDs) could withstand incorporation into the silica matrix and subsequent calcination at 500 °C for 2 h, the resulting 0.003 mg PP-CDs/SiO2 nanopowder was characterized using transmission electron microscopy (TEM) and X-ray photoelectron spectroscopy (XPS). These analyses were used to assess the nanoscale morphology and chemical composition of the material after thermal treatment. As shown in Fig. 3, the TEM image reveals nanoscale features distributed throughout the silica matrix, without noticeable aggregation. The measured average particle size was approximately 3.0 nm, smaller than that of the pristine PP-CDs. The XPS survey spectrum (Fig. 4) confirms the presence of C, N, O, and Si in the calcined composite. Furthermore, compared with pristine PP-CDs, the O 1s peaks of the PP-CDs/SiO2 composite exhibit a slight shift toward lower binding energies (Fig. 4c). This shift may be associated with changes in the local chemical environment of oxygen atoms resulting from interactions between silica network and oxygen-containing functional groups (–OH and –COOH) on the PP-CD surfaces during sol–gel processing and subsequent thermal treatment.35 The Si 2p spectrum (Fig. 4e) displayed two characteristic peaks corresponding to Si–O (103.16 eV) and C–Si (104.14 eV) bonding configurations.59 Collectively, the TEM and XPS results provide evidence that carbon-containing species remain incorporated within the silica matrix after calcination and that the composite exhibits changes in its nanoscale morphology and surface chemical environment.
Fig. 3. HR-TEM image of SiO2-0.003 PP-CDs nanopowder prepared by sol–gel method followed by calcination at 500 °C for 2 h.

Fig. 4. (a) Full scan XPS, high resolution spectra of (b) C 1s (c) O 1s (d) N 1s and (e) Si 2p of SiO2-0.003 PP-CDs prepared by sol–gel method followed by calcination at 500 °C for 2 h.

3.2. Characterization of SiO2-PP-CDs coated steel
The surface morphology, chemical composition, wettability, and nanoscale topography of uncoated S304 stainless steel and sol–gel derived SiO2 and SiO2-PP-CDs coatings before and after immersion in 1.0 M HCl for 24 h were systematically investigated using SEM, EDS, contact angle measurements, and AFM. All coating samples were calcinated at 500 °C to remove residual solvent and organics and to densify the silica network.60 Together, these results describe how PP-CD incorporation changes the coating morphology and its behavior after immersion.
Fig. 5a–d shows the X-ray diffraction (XRD) patterns of the uncoated 304 stainless steel (S304) (a) substrate and S304 coated with sol–gel derived SiO2 nanocomposite coating containing different PP-CDs loadings S304-SiO2 (b), S304-SiO2-0.003PP-CDs (c), and S304-SiO2-0.005PP-CDs (d).
Fig. 5. X-ray diffraction (XRD) patterns of the S304 (a), S304-SiO2 (b), S304-SiO2-0.003PP-CDs (c), and S304-SiO2-0.005PP-CDs (d) calcination at 500 °C.

The XRD pattern of the untreated S304 substrate exhibits two prominent diffraction peaks at 2θ = 43.57° and 50.51°, corresponding to the (111) and (200) planes of the face-centered cubic (FCC) γ-austenite phase (PDF card no. 33-0397), consistent with the characteristic crystalline structure of the stainless steel substrate.61
After coating deposition and calcination at 500 °C for 2 h, the characteristic γ-austenite reflections remain visible, accompanied by additional peaks at 2θ = 44.61° and 64.68°. These additional reflections may be consistent with the (110) and (200) planes of the α′-martensite phase (PDF card no. 19-0626). However, the available XRD data do not conclusively establish the presence of α′-martensite or confirm a γ → α′ martensitic transformation induced by the thermal treatment.62–65 Accordingly, this phase assignment is considered tentative and requires further phase-sensitive characterization for confirmation.62–65 Furthermore, all SiO2-based composite coatings exhibit a broad diffuse scattering halo centered at approximately 2θ = 22.04°, characteristic of amorphous silica-based materials.34 Although the position of the amorphous halo remains essentially unchanged, its intensity increases progressively with increasing PP-CD content.
Fig. 6a–d presents the SEM micrographs of the bare S304, S304-SiO2, S304-SiO2-0.003PP-CDs and S304-SiO2-0.005PP-CDs coatings before immersion in the 1.0 M HCl at 25 °C. The SEM observations before immersion reveal a clear evolution in surface structure with coating composition. The uncoated S304 stainless steel shows a smooth, mechanically polished surface with well-defined grinding marks and no signs of corrosion, confirming a clean baseline state (Fig. 6a). In contrast, the undoped SiO2 coating (S304-SiO2) exhibits a heterogeneous and appears composed of irregular silica agglomerates,34 interparticle voids, and microcracks. The average silica grain size is 120 nm. Similar features have been reported sol–gel derived silica films,34 where they are commonly attributed to rapid hydrolysis and condensation of silanol species leading to uncontrolled nucleation and aggregation (Fig. 6b).
Fig. 6. SEM images of the S304 substrate (a), S304-SiO2 (b), S304-SiO2-0.003PP-CDs (c), and S304-SiO2-0.005PP-CDs (d) calcination at 500 °C before immersion into 1.0 M HCl.

With the addition of 0.003 mg PP-CDs (S304-SiO2-0.003PP-CDs) (Fig. 6c), the coating morphology changes markedly compared with the undoped coating. The surface appears as a continuous film of closely packed grains, with no visible cracks or pores. Bright dots with an average diameter of ∼3.4 nm (Fig. 6c) are observed within the matrix and are tentatively assigned to PP-CDs; no agglomeration was observed in the imaged regions. The improved microstructure may be attributed to interactions between PP-CD functional groups and silica network species during So-gel process, which could regulate hydrolysis and condensation reactions. This is consistent with previous reports stating that carbon dots may act as nanoscale growth regulators (capping), limiting particle coalescence and promoting the formation of a refined and compact silica network.35
At higher loading (0.005 mg PP-CDs (S304-SiO2-0.005PP-CDs)) (Fig. 6d), the coating remains continuous with average grain size of 35 nm. Bright dots with an average diameter of ∼2.6 nm are observed on the surface of the silica film. They are distributed irregularly, with some agglomeration, and are tentatively assigned to PP-CDs. Compared with the 0.003 mg coating, a slight increase in surface heterogeneity and minor irregularities are observed. This may reflect a partial disruption of the condensation reactions, possibly caused by agglomerated PP-CD that leave fewer reactive silanol groups available (saturation).35
After immersion in 1.0 M HCl, the uncoated S304 substrate exhibits severe localized corrosion, characterized by widespread micropitting and surface degradation (Fig. 7a). This is consistent with the breakdown of the passive oxide layer and became attack by H+ and Cl− ions. The undoped SiO2 coating undergoes extensive failure, including cracking, delamination, and coating detachment (Fig. 7b). In contrast, the SiO2-0.003PP-CDs coating appears largely intact after immersion (Fig. 7c). Only minor scratches and isolated defects are observed, and no cracking or delamination was seen in the image. This intact surface after 24 h is consistent with the improved corrosion resistance measured electrochemically in the next section (Section 3.3). The SiO2-0.005PP-CDs coating also retains its continuity after immersion, but moderate surface roughening and localized bright deposits appear across the surface (Fig. 7d).
Fig. 7. SEM images of the S304 substrate (a), S304-SiO2 (b), S304-SiO2-0.003PP-CDs (c), and S304-SiO2-0.005PP-CDs (d) calcination at 500 °C after immersion into 1.0 M HCl for 24 h at 25 °C.

EDS analysis confirmed the presence of a silica-based coating on the S304 stainless steel substrate (Fig. 8). The spectrum of the bare S304 substrate shows the characteristic signals of Fe, Cr, Ni, O, and C (Fig. 8a). After coating deposition, a Si signal appears and the oxygen content increased relative to the bare substrate, which is consistent the deposited silica (Fig. 8b and d). The Fe, Cr, and Ni signals remain prominent, with a slight decrease in their atomic percentages. The carbon content of the S304-SiO2-0.003PP-CDs coating does not differ significantly from that of the undoped coating (Fig. 8b and d). This may be due to the low PP-CDs concentration, which is below the sensitivity of EDS for light elements.
Fig. 8. The EDS spectra of the S304 substrate (a), S304-SiO2 (b) and (c), S304-SiO2-0.003PP-CDs (d) and (e) calcination at 500 °C before and after immersion into 1.0 M HCl (24 h at 25 °C).

After immersion in 1.0 M HCl (25 °C, 24 h), the two coating show different compositional changes. For the undoped S304-SiO2 coating, the atomic percentages of the substrate elements, particularly Fe, differ markedly relative to the pre-immersion values (Fig. 8c), whereas the SiO2-0.003PP-CDs coating shows only a slight change, and its composition remains closer to the pre-immersion state (Fig. 8c). The oxygen content increases after immersion, which has been attributed in the literature to oxygen-containing species, potentially including oxygen-rich corrosion products.36 The 0.003 mg coating shows a lower relative chlorine signal than the undoped coating (Fig. 8), which has been related in previous reports to reduced accumulation of chloride species on the substrate surface.36 Because EDS is semi-quantitative, these differences in atomic content are treated as supporting, comparative observations and are not taken as the sole evidence of substrate dissolution or corrosion. The interpretation is substantiated by complementary evidence from the characterization and electrochemical results.
Contact angle measurements are consistent with these findings (Fig. 9). The uncoated S304 surface shows a contact angle of 65.75°, which decreases to 52.75° after immersion (−13.0°). This increase in wettability is consistent with the passive film breakdown and pitting seen in SEM. The undoped SiO2 coating (S304-SiO2) has a slightly higher initial contact angle (69.65°), which decreases to 60.75° after immersion (−8.9°); this may reflect the coating damage suggested from SEM. The S304-SiO2-0.003PP-CDs coating exhibits the smallest change, from 76.85° to 73.50° (−3.4°). This is consistent with a more intact surface as observed from SEM image. The S304-SiO2-0.005PP-CDs coating has the highest initial contact angle (77.30°). Its contact angle decreases more after immersion (to 68.50°, −8.8°), which may be related to the localized deposits and surface roughening observed in SEM (Fig. 7d).
Fig. 9. The static contact angle photographs of the S304 substrate (a) and (b) and S304-SiO2 (c) and (d), S304-SiO2-0.003PP-CDs (e) and (f), and S304-SiO2-0.005PP-CDs (g) and (h) before and after immersion into 1.0 M HCl (24 h at 25 °C).

AFM (Fig. 10) is consistent with these trends at the nanoscale. The roughness of the uncoated S304 surface increased after immersion, from Ra = 21.029 nm and Rrms = 26.411 nm to Ra = 33.660 nm and Rrms = 40.123 nm, in line with the pitting observed by SEM (Fig. 7a). The S304-SiO2-0.003PP-CDs coating was initially rougher (Ra = 44.863 nm, Rrms = 52.479 nm), which may be related to its nanostructured morphology, and after immersion Ra and Rrms decreased to 33.507 and 42.918 nm.
Fig. 10. AFM images of the S304 substrate (a) and (b) and S304-SiO2-0.003PP-CDs (c) and (d) calcinated at 500 °C before and after immersion into 1.0 M HCl (24 h at 25 °C).

3.3. Electrochemical measurements
3.3.1. Open circuit potential
The OCP profiles of uncoated and coated S304 in 1.0 M HCl at 25 °C are presented in Fig. 11. The uncoated S304 exhibits an initial potential of approximately −0.38 V vs. SCE, which gradually shifts toward more negative values, reaching about −0.42 V after 600 s. This negative shift may be attributed to changes in the metal/electrolyte interface during exposure to the acidic solution and the progressive stabilization of the interfacial conditions. In comparison, the S304-SiO2 sample exhibits a relatively stable OCP around −0.39 V throughout the measurement period, indicating a comparatively stable electrode/electrolyte interface.66
Fig. 11. OCP and EFM of S304 in a 1.0 M HCl with S304 substrate (a), S304-SiO2 (b), S304-SiO2-0.005PP-CDs (c), and S304-SiO2-0.003PP-CDs (d) at 25 °C.

The incorporation of PP-CDs into the SiO2 sol–gel matrix results in noticeable changes in the OCP evolution. The S304-SiO2-0.003PP-CDs coating shows a gradual shift toward more negative potentials, whereas the S304-SiO2-0.005PP-CDs coating initially exhibits the most positive OCP, followed by a gradual shift and stabilization near −0.39 V. These variations in OCP indicate that incorporation of PP-CDs modifies the interfacial characteristics of the SiO2 coating and its interaction with the acidic electrolyte. The differences in the OCP profiles may be related to changes in the coating microstructure, surface characteristics, and the accessibility of the electrolyte to the coated steel surface. Overall, the relatively stable OCP values observed for the coated specimens suggest that the coatings establish relatively stable interfacial conditions during immersion in 1.0 M HCl.67
3.3.2. Electrochemical frequency modulation (EFM)
The EFM measurements were performed by applying a sinusoidal perturbation containing two frequencies to the electrochemical system. The resulting current response contains harmonic and intermodulation components, which were analyzed to determine the corrosion current density (icorr) and the anodic and cathodic Tafel slopes (βa and βc). The corrosion parameters were obtained from the amplitudes of the characteristic intermodulation frequencies according to the standard EFM calculation procedure.
The electrochemical frequency modulation (EFM) spectra of uncoated and coated S304 specimens immersed in 1.0 M HCl at 25 °C are shown in Fig. 11. The spectra exhibit well-defined intermodulation peaks at the characteristic frequencies of the applied perturbation, confirming the nonlinear electrochemical response of the investigated systems.68 The EFM data obtained from these spectra are summarized in Table 1. For the uncoated S304, a relatively high corrosion current density icorr of 65.72 µA cm−2 was obtained, accompanied by a corrosion rate of 30.03 mpy. After modification of the steel surface with the SiO2-PP-CDs coatings, icorr decreased markedly to 32.59, 18.85, and 9.469 µA cm−2 for S304-SiO2, S304-SiO2-0.005PP-CDs, and S304-SiO2-0.003PP-CDs, respectively. Correspondingly, the corrosion rate decreased from 30.03 mpy for the uncoated specimen to 14.89, 8.615, and 4.327 mpy, respectively. This progressive decrease in icorr demonstrates that the coatings effectively suppress the electrochemical corrosion reactions occurring on the S304 surface.
Table 1. Electrochemical frequency modulation (EFM) parameters obtained for S304 corrosion in a 1.0 M HCl solution without and with studied compounds at 25 °C.
| Compounds | i corr/µA cm−2 | β a (mV dec−1) | −βc (mV dec−1) | C.R (mpy) | CF-2 | CF-3 | η EFM% |
|---|---|---|---|---|---|---|---|
| Uncoated S304/HCl | 65.72 ± 0.52 | 116.1 ± 0.32 | 157.6 ± 0.90 | 30.03 ± 0.02 | 2.121 ± 0.06 | 2.39 ± 0.02 | — |
| S304-SiO2/HCl | 32.59 ± 0.72 | 136.3 ± 0.32 | 188.7 ± 0.37 | 14.89 ± 0.87 | 2.209 ± 0.01 | 2.301 ± 0.02 | 50.41 ± 0.31 |
| S304-SiO2-0.005PP-CDs/HCl | 18.85 ± 0.30 | 120.5 ± 0.52 | 185.1 ± 0.07 | 8.615 ± 0.10 | 2.044 ± 0.01 | 1.961 ± 0.02 | 71.32 ± 0.10 |
| S304-SiO2-0.003PP-CDs/HCl | 9.469 ± 0.20 | 114.3 ± 0.41 | 174.8 ± 0.65 | 4.327 ± 0.10 | 2.106 ± 0.03 | 2.987 ± 0.10 | 85.59 ± 0.47 |
The inhibition efficiencies (ηEFM%) calculated69 from the EFM measurements, eqn (1),70 were 50.41%, 71.32%, and 85.59% for S304-SiO2, S304-SiO2-0.005PP-CDs, and S304-SiO2-0.003PP-CDs, respectively. Where i0corr and icorr are the values of corrosion current density for S304 in the absence and presence of SiO2-PP-CDs, respectively. The highest inhibition efficiency was therefore obtained for the S304-SiO2-0.003PP-CDs coating, indicating that the incorporation of the appropriate amount of PP-CDs substantially improves the protective performance of the SiO2 coating. The enhanced inhibition can be attributed to the formation of a more effective and compact protective layer that limits the access of aggressive H+ and Cl− species to the steel/electrolyte interface. The PP-CDs may also provide additional active sites and improve the barrier properties and interfacial interaction of the coating with the metal surface.
![]() |
1 |
The EFM spectra provide further evidence for this protective effect. Compared with the uncoated S304, the coated specimens exhibit changes in the amplitude and distribution of the intermodulation peaks, reflecting a reduction in the rate of the electrochemical corrosion reactions. The decrease in the EFM-derived icorr is consistent with the improved corrosion resistance produced by the SiO2-PP-CDs coatings.
On the other hand, an important advantage of the EFM technique is that the validity of the obtained electrochemical parameters can be assessed using the causality factors (CF-2 and CF-3). At different concentrations, the experimental values for the investigated specimens are close to their theoretical values of 2 and 3, respectively, which are the theoretical values expected for a reliable EFM measurement.69Table 1 showed that, CF-2 values ranged from 2.044 to 2.209, while CF-3 values ranged from 1.961 to 2.987 for the coated specimens. The slight deviations from the ideal values can be attributed to the complexity and nonlinearity of the electrochemical processes occurring at the coated steel/electrolyte interface.
The corrosion parameters obtained by EFM therefore demonstrate that the SiO2-PP-CDs nanocomposite coating significantly reduces the corrosion activity of S304 in 1.0 M HCl, with the S304-SiO2-0.003PP-CDs system showing the most pronounced protective effect. The EFM results are in good agreement with the observed reduction in corrosion current density and corrosion rate, supporting the conclusion that PP-CD incorporation enhances the barrier and corrosion-inhibition properties of the SiO2 coating.
3.3.3. Electrochemical impedance spectroscopy (EIS)
The electrochemical impedance spectroscopy (EIS) results for uncoated and SiO2-PP-CDs-coated S304 specimens immersed in 1.0 M HCl at 25 °C are presented in Fig. 12, while the corresponding electrochemical parameters are listed in Table 2. The experimental impedance spectra were satisfactorily fitted using the equivalent electrical circuit shown in Fig. 13, consisting of the solution resistance (Rs) and two time constants represented by Rct/CPEdl and Rf/CPEf. Here, Rct represents the charge-transfer resistance at the metal/electrolyte interface,71 whereas Rf is associated with the resistance of the protective coating layer. The CPE elements account for the non-ideal capacitive behavior resulting from surface roughness, coating heterogeneity, porosity, and non-uniform distribution of electrochemical properties.72
Fig. 12. Nyquist, Bode modulus, and Bode phase plots of S304 in a 1.0 M HCl with S304 substrate (a), S304-SiO2 (b), S304-SiO2-0.005PP-CDs (c), and S304-SiO2-0.003PP-CDs (d) at 25 °C.

Table 2. Electrochemical impedance spectroscopy (EIS) parameters obtained for S304 corrosion in a 1.0 M HCl solution without and with studied compounds at 25 °C.
| Compounds | R s/Ω cm2 | R ct × 103/Ω cm2 | R f/Ω cm2 | R P × 103/Ω cm2 | CPEdl × 10−5 (Ω−1 cm−2 sn1) | CPEf × 10−5 (Ω−1 cm−2 sn2) | n 1 × 10−1 | n 2 × 10−1 | η EIS% | X 2 × 10−3 |
|---|---|---|---|---|---|---|---|---|---|---|
| Uncoated S304/HCl | 9.838 ± 0.09 | 2.03 ± 0.1 | 16.7 ± 0.18 | 2.04 ± 0.03 | 4.39 ± 0.02 | 5.97 ± 0.03 | 8.01 ± 0.09 | 7.97 ± 0.03 | — | 0.746 ± 0.01 |
| S304-SiO2/HCl | 35.88 ± 0.11 | 2.42 ± 0.02 | 374.2 ± 0.08 | 2.79 ± 0.01 | 5.58 ± 0.06 | 0.335 ± 0.01 | 9.99 ± 0.07 | 8.35 ± 0.01 | 26.88 ± 0.10 | 1.10 ± 0.01 |
| S304-SiO2-0.005PP-CDs/HCl | 11.65 ± 0.02 | 3.72 ± 0.01 | 23.63 ± 0.01 | 3.74 ± 0.03 | 3.41 ± 0.06 | 9.94 ± 0.02 | 6.62 ± 0.05 | 9.94 ± 0.01 | 45.48 ± 0.07 | 2.16 ± 0.05 |
| S304-SiO2-0.003PP-CDs/HCl | 8.922 ± 0.04 | 4.84 ± 0.01 | 527.6 ± 0.08 | 5.37 ± 0.01 | 6.15 ± 0.02 | 0.891 ± 0.01 | 9.8 ± 0.01 | 8.91 ± 0.02 | 62.01 ± 0.10 | 2.08 ± 0.11 |
Fig. 13. Equivalent circuit used to model metal/solution interface of S304 in a 1.0 M HCl with S304 substrate (a), S304-SiO2 (b), S304-SiO2-0.005PP-CDs (c), and S304-SiO2-0.003PP-CDs (d) at 25 °C.

The Nyquist plots show depressed capacitive loops for all investigated specimens, indicating the heterogeneous nature of the S304/electrolyte interface.73 Compared with the uncoated specimen, the coated samples generally exhibit a larger impedance response, particularly for the S304-SiO2–0.003PP-CDs system. This behavior indicates an increase in the resistance to charge transfer and/or ionic transport through the protective coating, thereby confirming the beneficial effect of the SiO2-PP-CDs coating.
For the uncoated S304, the Rct value was only 2.03 × 103 Ω cm2, while the coating resistance (Rf) was 16.7 cm2, giving a total polarization resistance (RP) of approximately 2.04 × 103 Ω cm2. Upon coating the steel with SiO2-PP-CDs, (RP) increased to 2.79 × 103, 3.74 × 103, and 5.37 × 103 Ω cm2 for S304-SiO2, S304-SiO2-0.005PP-CDs, and S304-SiO2-0.003PP-CDs, respectively. The progressive increase in RP demonstrates that the coating provides an effective barrier against the penetration of the aggressive HCl electrolyte toward the steel surface.
The inhibition efficiency of SiO2-PP-CDs, ηEIS%, for the S304 electrode can be measured as follows: eqn (2).74
![]() |
2 |
where
and RP are the polarization resistances for uninhibited and inhibited 1.0 M HCl solutions, respectively, and RP is a sum of Rf and Rct.
The EIS inhibition efficiencies (ηEIS%)75 were 26.88%, 45.48%, and 62.01% for S304-SiO2, S304-SiO2-0.005PP-CDs, and S304-SiO2-0.003PP-CDs, respectively. Thus, the S304-SiO2-0.003PP-CDs coating exhibited the highest impedance-based protection, which is consistent with its highest RP value. The increase in RP can be attributed to the formation of a more effective and less permeable coating layer that hinders the transport of corrosive species.
Interestingly, the contribution of the coating resistance (Rf) is particularly evident for the S304-SiO2-0.005PP-CDs sample. Although its Rct value (3.72 × 103 Ω cm2) is relatively low, its Rf reaches 23.63 Ω cm2, resulting in a relatively high RP of 3.74 × 103 Ω cm2. This suggests that, for this composition, the protective behavior is dominated by the barrier effect of the coating film rather than by a large increase in the interfacial charge-transfer resistance. In contrast, the S304-SiO2-0.003PP-CDs coating combines a high Rct (4.84 × 103 Ω cm2) with the highest Rf (527.6 Ω cm2), providing the strongest overall resistance to the corrosion process.
The CPE parameters also provide information about the interfacial properties. The n1 values range from 0.662 to 0.999, while n2 values range from 0.797 to 0.994, confirming the non-ideal capacitive behavior of the interfaces. Such deviations from ideal capacitive behavior are commonly associated with surface heterogeneity, roughness, non-uniform current distribution, and the presence of a protective coating. The variation in CPE values after coating further indicates modification of the electrical properties of the metal/electrolyte interface.22
On the other hand, the Bode modulus plots provide additional evidence for the protective action of the coatings. The coated specimens exhibit higher impedance magnitudes over a broad frequency range, with the S304-SiO2-0.003PP-CDs system showing the most pronounced impedance response. A higher low-frequency impedance magnitude reflects a greater resistance of the electrochemical system to corrosion reactions. The Bode phase plots also show changes in the phase-angle response after coating, reflecting modification of the interfacial electrochemical processes and the contribution of the coating layer.
The quality of the EIS fitting was assessed using the chi-square (X2) statistic obtained from the equivalent-circuit fitting procedure. The (X2) values were (0.746, 1.10, 2.16, and 2.08) × 10−3 for the uncoated S304/HCl, S304-SiO2/HCl, S304-SiO2-0.005PP-CDs/HCl, and S304-SiO2-0.003PP-CDs/HCl systems, respectively. The experimental and fitted impedance spectra showed good agreement over the investigated frequency range, supporting the suitability of the selected equivalent circuit for describing the electrochemical response of the investigated systems.
Finally, the EIS results demonstrate that incorporation of PP-CDs into the SiO2 coating significantly improves the corrosion resistance of S304 in 1.0 M HCl. Among the investigated coatings, S304-SiO2-0.003PP-CDs provide the optimum protective performance. The improvement is attributed primarily to the formation of a more effective barrier layer that limits electrolyte penetration and suppresses the electrochemical corrosion reactions at the steel/coating/electrolyte interface. These EIS findings are also consistent with the EFM results, where the same coating exhibited the lowest icorr and highest inhibition efficiency.
3.3.4. Potentiodynamic polarization (PDP)
The potentiodynamic polarization measurements were performed over a potential range of −1000 to +1000 mV relative to the open-circuit potential (OCP). This relatively wide potential window was selected to obtain well-defined cathodic and anodic branches around the corrosion potential, allowing reliable determination of the corrosion potential (Ecorr) and corrosion current density (icorr) from the corresponding Tafel regions. The selected range also provides sufficient polarization to characterize both the cathodic hydrogen evolution and anodic metal dissolution processes. It should be noted that polarization at potentials far from (Ecorr) may cause some irreversible changes at the electrode/coating-electrolyte interface. Therefore, the PDP measurements were primarily used for electrochemical characterization and determination of corrosion parameters rather than for non-destructive assessment of the surface condition. The interpretation of the protective performance was supported by complementary electrochemical and surface characterization techniques.
The potentiodynamic polarization curves of uncoated and SiO2-PP-CDs-coated S304 specimens in 1.0 M HCl at 25 °C are presented in Fig. 14. The polarization curves provide information about the influence of the coatings on both the anodic metal dissolution and cathodic hydrogen evolution reactions.
Fig. 14. Potentiodynamic polarization curves of S304 in a 1.0 M HCl with S304 substrate (a), S304-SiO2 (b), S304-SiO2-0.005PP-CDs (c), and S304-SiO2-0.003PP-CDs (d) at 25 °C.

The corrosion potential (Ecorr), corrosion current density (icorr), and anodic and cathodic Tafel slopes (βa and βc) were determined from the potentiodynamic polarization curves using Tafel extrapolation. The linear portions of the anodic and cathodic branches were selected for fitting based on their approximately linear relationship between the potential and log i. Regions showing significant curvature or deviation from linear Tafel behavior were excluded from the fitting. The intersection of the extrapolated anodic and cathodic Tafel lines was used to determine (Ecorr) and (icorr), while the slopes of the corresponding linear regions were used to obtain βa and βc. For the SiO2-PP-CDs-coated S304 specimens, the Tafel-derived parameters were interpreted with caution because coating resistance, surface heterogeneity, and changes in charge-transfer kinetics can cause deviations from ideal Tafel behavior. Therefore, the (icorr) values obtained from Tafel extrapolation were considered primarily as comparative electrochemical parameters rather than absolute measurements of uniform corrosion rates. The PDP results were consequently evaluated together with the EIS, EFM, and surface characterization results.
As shown in Fig. 14, the polarization behavior of the coated specimens differs from that of the uncoated S304, indicating that the SiO2-PP-CDs coatings effectively modify the electrochemical reactions occurring at the steel/electrolyte interface.76 The curves show changes in both the anodic and cathodic branches, suggesting that the coatings suppress the overall corrosion process by limiting the interaction between the aggressive HCl solution and the steel surface.
For the uncoated S304, relatively high cathodic and anodic current densities are observed, reflecting the relatively rapid corrosion reactions in the acidic medium. After coating, the current densities of both branches are generally reduced, particularly for the S304-SiO2-0.003PP-CDs system (Table 3). This decrease in current density indicates that the coating acts as an effective barrier, restricting the transport of corrosive species toward the metal surface and consequently reducing both the anodic dissolution of iron and the cathodic hydrogen evolution reaction.
Table 3. Potentiodynamic polarization (PDP) parameters obtained for S304 corrosion in a 1.0 M HCl solution without and with studied compounds at 25 °C.
| Compounds | i corr (µA cm−2) | −Ecorr (mVSCE) | β a (mV dec−1) | −βc (mV dec−1) | C.R (mpy) | η Pot.% |
|---|---|---|---|---|---|---|
| Uncoated S304/HCl | 87.3 ± 0.20 | 419 ± 0.41 | 2192 ± 0.01 | 2479 ± 0.01 | 39.91 ± 0.04 | — |
| S304-SiO2/HCl | 41.2 ± 0.30 | 444 ± 1.47 | 168.3 ± 0.29 | 181.7 ± 0.61 | 18.84 ± 0.03 | 52.81 ± 0.42 |
| S304-SiO2-0.005PP-CDs/HCl | 22.4 ± 0.11 | 457 ± 0.83 | 173.2 ± 0.13 | 220.4 ± 0.32 | 10.23 ± 0.02 | 74.34 ± 0.06 |
| S304-SiO2-0.003PP-CDs/HCl | 13.8 ± 0.11 | 425 ± 0.82 | 229.4 ± 0.36 | 182.8 ± 0.75 | 6.326 ± 0.01 | 84.19 ± 0.01 |
The polarization curves also indicate that the addition of PP-CDs does not cause a pronounced displacement of the corrosion potential toward either strongly anodic or strongly cathodic values. Therefore, the SiO2-PP-CDs coatings can be considered to provide a mixed-type protective effect, affecting both anodic and cathodic corrosion reactions rather than selectively inhibiting only one partial reaction.77
The inhibition efficiency ηPot.% was calculated from the following equation:
![]() |
3 |
where i0corr and icorr are the values of corrosion current density for S304 in the absence and presence of SiO2-PP-CDs, respectively.78
Among the investigated coatings, S304-SiO2-0.003PP-CDs exhibit the most significant suppression of the polarization currents, confirming its superior protective performance. This observation agrees with the EIS results, where this coating exhibited the highest polarization resistance. It is also consistent with the EFM results, which showed the lowest corrosion current density and the highest inhibition efficiency for the same coating.
The enhanced protection provided by the optimum PP-CDs loading can be attributed to the formation of a more compact and effective SiO2-PP-CDs nanocomposite layer on the S304 surface. Generally, the PDP results confirm that incorporation of PP-CDs enhances the protective ability of the SiO2 coating, with the 0.003 PP-CDs loading providing the most effective corrosion protection for S304 in 1.0 M HCl at 25 °C.
3.4. Correlation between coating microstructure and corrosion-protection performance: comparative assessment by EFM, EIS and PDP and proposed inhibition mechanism
Fig. 15 compares the inhibition efficiencies of the SiO2-PP-CDs coatings calculated using electrochemical frequency modulation (EFM), electrochemical impedance spectroscopy (EIS) and potentiodynamic polarization (PDP), with uncoated S304 as the reference. All three techniques indicate a consistent improvement in the corrosion protection of S304 following coating deposition and PP-CD incorporation, and give the same ranking of the coatings, S304-SiO2 < S304-SiO2-0.005PP-CDs < S304-SiO2-0.003PP-CDs. The S304-SiO2-0.003PP-CDs coating shows the highest inhibition efficiency of all compositions, indicating that an appropriate PP-CD loading is essential for optimal protection.
Fig. 15. Inhibition efficiency values calculated from EFM (a), EIS (b), and PDP (c) methods for the coated S304 samples in a 1.0 M HCl solution. Error bars represent the standard deviation at 25 °C.

The relationship between coating morphology and corrosion-protection performance was evaluated by combining SEM observations, contact-angle measurements, and electrochemical results obtained from EFM, EIS, and PDP. Before immersion, the S304-SiO2-0.003PP-CDs coating exhibited a relatively continuous surface morphology without visible cracks or pores in the examined SEM regions. After immersion in 1.0 M HCl for 24 h at 25 °C, this coating largely retained its morphological integrity, with only minor scratches and isolated defects and no visible cracking or delamination in the examined regions. In contrast, the undoped SiO2 coating exhibited pronounced cracking and delamination after immersion, while the coating containing 0.005 mg of PP-CDs showed moderate surface roughening and localized bright deposits. These differences in the observed surface morphology were accompanied by changes in wettability. The contact angle of the S304-SiO2-0.003PP-CDs coating decreased only slightly, from 76.85° to 73.50° (a decrease of 3.35°), whereas the undoped SiO2 coating decreased from 69.65° to 60.75° (8.90°), and the coating containing 0.005 mg of PP-CDs decreased from 77.30° to 68.50° (8.80°). The smaller contact-angle change for the 0.003 mg formulation indicates better retention of its initial wettability after acid exposure.
The electrochemical measurements further support this trend. The inhibition efficiencies of the undoped SiO2 coating were 50.41%, 26.88%, and 52.81%, as determined by EFM, EIS, and PDP, respectively. Increasing the PP-CD loading to 0.005 mg improved these values to 71.32%, 45.48%, and 74.34%, respectively. The highest efficiencies were obtained for the S304-SiO2-0.003PP-CDs coating, reaching 85.59% by EFM, 62.01% by EIS, and 84.19% by PDP. Consistently, the EFM-derived corrosion current density decreased from 65.72 for uncoated S304 to 32.59 for the undoped SiO2 coating, 18.85 for the 0.005 mg PP-CD formulation, and 9.469 for the 0.003 mg formulation (in the units reported in Table 1). Thus, all three electrochemical techniques identified the 0.003 mg formulation as the most effective among the investigated coatings. The agreement between the morphological, wettability, electrochemical results suggests that the improved protection is associated with PP-CD incorporation together with the accompanying changes in coating morphology and surface characteristics. The relatively continuous surface and smaller change in contact angle observed for the 0.003 mg coating are consistent with a coating that better limits electrolyte access to the S304 Nevertheless, pore blocking, coating densification, and increased diffusion-path tortuosity were not directly quantified in this study and should therefore be regarded as possible explanations rather than experimentally confirmed mechanisms. The individual contributions of PP-CD incorporation and the associated morphological changes cannot be conclusively separated using the available data.
3.5. Proposed corrosion mechanism
Based on these results, the following mechanism is proposed as an interpretation. In the undoped coating, microcracks and voids may act as pathways for H+ and Cl− to reach the steel, consistent with its cracking and delamination after immersion (Fig. 7b). At 0.003 mg, PP-CDs carrying hydroxyl, carbonyl and carboxyl groups (Section 3.1) may interact with silanol groups of the sol–gel network during hydrolysis and polycondensation steps,35 as suggested by the shift of the O 1s peaks in the calcined composite powder. This may promote more uniform condensation and reduce the formation of cracks and voids, giving the continuous film observed, whose high Rf is consistent with a longer ion-diffusion path. At 0.005 mg, partial agglomeration of PP-CDs (Fig. 6d) may disturb film homogeneity and create local weak points.
From a practical standpoint, 1.0 M HCl is a strongly acidic, chloride-containing medium commonly used to simulate hydrochloric acid cleaning and descaling conditions, in which the passive film of stainless steel is destabilized.55–57 In this medium, the 0.003 mg coating remained essentially intact after 24 h and substantially reduced the corrosion rate of S304, as quantified above. These results suggest potential for protecting 304 stainless steel surfaces exposed to HCl-containing cleaning and process solutions, where slower metal loss could be beneficial under comparable short-term exposure. However, these findings come from laboratory coupons tested for 24 h at 25 °C.
4. Conclusion
Pomegranate-peel-derived carbon dots (PP-CDs) were incorporated into sol–gel silica coatings to improve the corrosion resistance of stainless steel 304 (S304) in 1.0 M HCl. The results demonstrated that the protective performance depended on the PP-CD loading, with the S304-SiO2-0.003PP-CDs coating exhibiting the best overall performance among the investigated formulations. After 24 h of immersion at 25 °C, this coating retained a largely continuous surface without visible cracking or delamination, whereas the undoped SiO2 coating exhibited pronounced cracking and delamination. Consistent with these morphological observations, the inhibition efficiencies determined by EFM, EIS, and PDP were 85.6%, 62.0%, and 84.2%, respectively, for the 0.003 mg PP-CD coating, compared with 50.4%, 26.88%, and 52.8% for the undoped SiO2 coating. The 0.005 mg PP-CD formulation showed intermediate corrosion-protection performance, accompanied by partial PP-CD agglomeration, highlighting the importance of optimizing the additive loading. The comparatively small change in contact angle after immersion further supported the retention of surface characteristics by the 0.003 mg coating. Collectively, the electrochemical and surface-characterization results suggest that the improved protection is associated with PP-CD incorporation and the accompanying changes in coating continuity and morphological uniformity. These findings demonstrate the potential of PP-CD-modified sol–gel silica coatings for protecting S304 against acidic attack under the short-term laboratory conditions investigated.
Author contributions
H. A. Siam: data curation; formal analysis; investigation; validation; writing – review and editing. R. Helmy: data curation; formal analysis: validation; visualization; writing – original draft; writing – review and editing. M. Saif: conceptualization; data curation; formal analysis; visualization; writing – original draft; writing – review and editing. Amr Gangan: formal analysis and validation. N. S. Abdelshafi: conceptualization; data curation; formal analysis; validation; writing – original draft; writing – review and editing. Hanan A. Soliman: data curation; formal analysis: validation; visualization; writing – original draft; writing-review and editing.
Conflicts of interest
There are no conflicts to declare.
Supplementary Material
Data availability
The datasets used and/or analyzed during the current study are available from the corresponding author on reasonable request.
Supplementary information (SI): the raw electrochemical data and curves obtained from the electrochemical techniques used in this study. See DOI: https://doi.org/10.1039/d6ra08713b.
References
- Loto R. T. Oladipupo S. Folarin T. Okosun E. Discover Appl. Sci. 2025;7:672–689. doi: 10.1007/s42452-025-07234-4. [DOI] [Google Scholar]
- Abdelhamid H. N. Eissa M. E. RSC Adv. 2026;16:14936–14950. doi: 10.1039/D5RA08536E. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Sheydaei M. Edraki M. J. Appl. Mater. Sci. 2025;1:210131–210142. [Google Scholar]
- Wang H. Dong L. Xue Y. Zhang J. An Y. Tribol. Int. 2026;224:112366–112383. doi: 10.1016/j.triboint.2026.112366. [DOI] [Google Scholar]
- Ćurković L. Ćurković H. O. Salopek S. Renjo M. M. Šegota S. Corros. Sci. 2013;77:176–184. doi: 10.1016/j.corsci.2013.07.045. [DOI] [Google Scholar]
- Huang J.-J. Wu M.-J. Hsu C.-F. Chen J.-Y. Surf. Coat. Technol. 2014;259:346–351. doi: 10.1016/j.surfcoat.2014.02.016. [DOI] [Google Scholar]
- Gecu R. Birol B. Özcan M. Trans. IMF. 2022;100:324–332. doi: 10.1080/00202967.2022.2117884. [DOI] [Google Scholar]
- Kim J.-H. Farithkhan A. Jung M.-J. Kwon S.-H. Coatings. 2026;16:55–66. doi: 10.3390/coatings16010055. [DOI] [Google Scholar]
- Zhang W. Ji G. Bu A. Zhang B. ACS Appl. Mater. Interfaces. 2015;7:28264–28272. doi: 10.1021/acsami.5b07915. [DOI] [PubMed] [Google Scholar]
- Xu Z. He Z. Wang Z. Zhang J. J. Mater. Eng. Perform. 2019;28:4983–4990. doi: 10.1007/s11665-019-04221-w. [DOI] [Google Scholar]
- de Paula Krasauskas L. R. de Oliveira L. A. de Oliveira M. C. L. Antunes R. A. J. Mater. Eng. Perform. 2026;35:21121–21133. doi: 10.1007/s11665-026-13609-4. [DOI] [Google Scholar]
- Kant S. Kumari N. Kumar M. Appl. Phys. A. 2025;131:631–647. doi: 10.1007/s00339-025-08755-w. [DOI] [Google Scholar]
- Spajić I. Rahimi E. Lekka M. Offoiach R. Fedrizzi L. Milošev I. J. Electrochem. Soc. 2021;168:071510–071525. doi: 10.1149/1945-7111/ac131b. [DOI] [Google Scholar]
- Cheng W. Li C. Ma X. Yu L. Liu G. Mater. Des. 2017;126:155–161. doi: 10.1016/j.matdes.2017.04.041. [DOI] [Google Scholar]
- Prasad V. J. S. N. Pamu D. Ceram. Int. 2026 doi: 10.1016/j.ceramint.2026.05.322. [DOI] [Google Scholar]
- Shin D. Kim K. Nam I.-T. Han S. Mater. Sci. Forum. 2006;510–511:442–445. [Google Scholar]
- Szczurek J. Gąsiorek A. Szczurek A. Babiarczuk B. Kowalski M. Karolczak P. Jones W. Wróblewski R. Adamek J. Maciej A. Kaleta J. Krzak J. Simka W. Surf. Coat. Technol. 2023;455:129220–129236. doi: 10.1016/j.surfcoat.2022.129220. [DOI] [Google Scholar]
- Nazeri A. Trzaskoma-Paulette P. P. Bauer D. J. Sol-Gel Sci. Technol. 1997;10:317–331. doi: 10.1023/A:1018381503008. [DOI] [Google Scholar]
- Mudali U. K. Sridhar T. M. Rajendran N. Surf. Eng. 2007;23:267–272. doi: 10.1179/174329407X215069. [DOI] [Google Scholar]
- Montemor M. F. Trabelsi W. Lamaka S. V. Yasakau K. A. Zheludkevich M. L. Bastos A. C. Ferreira M. G. S. Electrochim. Acta. 2008;53:5913–5922. doi: 10.1016/j.electacta.2008.03.069. [DOI] [Google Scholar]
- Ye J. Yu X. Bi W. Li D. Ma H. Zhao H. Qiu G. Wang L. Key Eng. Mater. 2008;368–372:1838–1840. [Google Scholar]
- Soliman H. A. Ibrahim M. M. Ali L. I. Saif M. Abdelshafi N. S. Khaled K. F. Moroccan J. Chem. 2023;11:780–801. [Google Scholar]
- Upadhyay V. Bergseth Z. Kelly B. Battocchi D. Coatings. 2017;7:86–97. doi: 10.3390/coatings7070086. [DOI] [Google Scholar]
- Gąsiorek J. Szczurek A. Babiarczuk B. Kaleta J. Jones W. Krzak J. Materials. 2018;11:197–215. doi: 10.3390/ma11020197. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Vasconcelos D. C. L. Carvalho J. A. N. Mantel M. Vasconcelos W. L. J. Non-Cryst. Solids. 2000;273:135–139. doi: 10.1016/S0022-3093(00)00155-1. [DOI] [Google Scholar]
- Vivar Mora L. Naik S. Paul S. Dawson R. Neville A. Barker R. Surf. Coat. Technol. 2017;324:368–375. doi: 10.1016/j.surfcoat.2017.05.063. [DOI] [Google Scholar]
- Wang D. Bierwagen G. P. Prog. Org. Coat. 2009;64:327–338. doi: 10.1016/j.porgcoat.2008.08.010. [DOI] [Google Scholar]
- Li J. Bai H. Feng Z. Molecules. 2023;28:2563–2593. doi: 10.3390/molecules28062563. [DOI] [PMC free article] [PubMed] [Google Scholar]
- He H. Zhang Z. Jiang C. He C. J. Mol. Struct. 2025;1334:141894–141912. doi: 10.1016/j.molstruc.2025.141894. [DOI] [Google Scholar]
- Li Q., in Corrosion Prevention of Magnesium Alloys, ed. G.-L. Song, Woodhead Publishing, Cambridge, UK, 2013, ch. 17, pp. 469–485, 10.1533/9780857098962.3.469 [DOI] [Google Scholar]
- Zakaria H. Liu M. Xiang L. Yang T. Hou Y. Yang X. Ding J. Zheng S. Hussain G. Domblesky J. P. Kong J. Shen G. Zhou L. Akhtar M. Wei H. Mater. Res. Bull. 2026;202:114169–114182. doi: 10.1016/j.materresbull.2026.114169. [DOI] [Google Scholar]
- Rai A. Szczerba M. Karbowniczek J. Cichocki K. Krzyzanowski M. Bajda S. Sulka G. D. Szuwarzyński M. Sokołowski K. Wiese B. Appl. Surf. Sci. 2025;695:162847–162860. doi: 10.1016/j.apsusc.2025.162847. [DOI] [Google Scholar]
- Duan X. Wang Y. Guo R. Niu B. Wang H. Yan H. Mater. Chem. Phys. 2025;330:130164–130175. doi: 10.1016/j.matchemphys.2024.130164. [DOI] [Google Scholar]
- Wu C. He J. Appl. Surf. Sci. 2026;715:164427–164435. doi: 10.1016/j.apsusc.2025.164427. [DOI] [Google Scholar]
- Seifzadeh D. Samadianfard R. Dikici B. Surf. Eng. 2024;40:742–757. doi: 10.1177/02670844241282605. [DOI] [Google Scholar]
- Mohamed M. E. Abd-El-Nabey B. A. Ezzat A. Sci. Rep. 2026;16:13897–13919. doi: 10.1038/s41598-026-47261-8. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Liu X. Li J. Li S. He C. He H. Nanomaterials. 2026;16:488–516. doi: 10.3390/nano16080488. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Mura S. Ludmerczki R. Stagi L. Garroni S. Carbonaro C. M. Ricci P. C. Casula M. F. Malfatti L. Innocenzi P. Sci. Rep. 2020;10:4770–4782. doi: 10.1038/s41598-020-61517-x. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Liu W. Li C. Ren Y. Sun X. Pan W. Li Y. Wang J. Wang W. J. Mater. Chem. B. 2016;4:5772–5788. doi: 10.1039/C6TB00976J. [DOI] [PubMed] [Google Scholar]
- Al Ragib A. Amin A. Alanazi Y. Kormoker T. Uddin M. Siddique M. Barai H. Carbon Res. 2023;2:1–30. [Google Scholar]
- Cao M. Li Y. Song X. Chen Y. Sun L. Shi X. Dai C. Yuan B. Fuel. 2023;352:129046–129057. doi: 10.1016/j.fuel.2023.129046. [DOI] [Google Scholar]
- Wu Y. Zheng Y. You F. Liu X. Zhang G. Carbon. 2026;249:121227–121241. doi: 10.1016/j.carbon.2026.121227. [DOI] [Google Scholar]
- Hong W. T. Yang H. K. Optik. 2021;241:166449–166457. doi: 10.1016/j.ijleo.2021.166449. [DOI] [Google Scholar]
- Li W. Han Y. Wang X. Zhao H. ACS Appl. Nano Mater. 2024;7:2304–2311. doi: 10.1021/acsanm.3c05760. [DOI] [Google Scholar]
- Lotey N. K. B. Lemos R. D'Silva F. Deshmukh A. Singh N. Wankhede S. Davuluri R. Vishe N. Kulkarni S. J. Fluoresc. 2025;35:7361–7371. doi: 10.1007/s10895-024-04107-8. [DOI] [PubMed] [Google Scholar]
- Jabeen S. Lin Y. Chen H. Li S. Chen S.-W. ji Y. Liu X. Chu J. Yu R. Spectrochim. Acta, Part A. 2026;357:127840–127851. doi: 10.1016/j.saa.2026.127840. [DOI] [PubMed] [Google Scholar]
- Kaur A. Pandey K. Kaur R. Vashishat N. Kaur M. Chemosensors. 2022;10:367–396. doi: 10.3390/chemosensors10090367. [DOI] [Google Scholar]
- Bortolami M. Curulli A. Di Matteo P. Petrucci R. Feroci M. Sensors. 2024;24:3945–3968. doi: 10.3390/s24123945. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Shi H. Wei J. Qiang L. Chen X. Meng X. J. Biomed. Nanotechnol. 2014;10:2677–2699. doi: 10.1166/jbn.2014.1881. [DOI] [PubMed] [Google Scholar]
- Boakye-Yiadom K. O. Kesse S. Opoku-Damoah Y. Filli M. S. Aquib M. Joelle M. M. B. Farooq M. A. Mavlyanova R. Raza F. Bavi R. Wang B. Int. J. Pharm. 2019;564:308–317. doi: 10.1016/j.ijpharm.2019.04.055. [DOI] [PubMed] [Google Scholar]
- Mathew J. Mathew B. Microchem. J. 2026;227:118910–118921. doi: 10.1016/j.microc.2026.118910. [DOI] [Google Scholar]
- Park S. J. Yang H. K. Curr. Appl. Phys. 2022;36:9–15. doi: 10.1016/j.cap.2022.01.001. [DOI] [Google Scholar]
- Etefa H. F. Dejene F. B. New Carbon Mater. 2026;41:253–275. doi: 10.1016/S1872-5805(26)61074-8. [DOI] [Google Scholar]
- Sattariazar S. Arsalani N. Nejad Ebrahimi S. Mater. Chem. Phys. 2023;294:126981–126989. doi: 10.1016/j.matchemphys.2022.126981. [DOI] [Google Scholar]
- Li L.-F. Caenen P. Celis J.-P. Corros. Sci. 2008;50:804–810. doi: 10.1016/j.corsci.2007.09.006. [DOI] [Google Scholar]
- Oguike R. Adv. Mater. Phys. Chem. 2014;4:153–163. doi: 10.4236/ampc.2014.48018. [DOI] [Google Scholar]
- Zatkalíková V. Uhríčik M. Markovičová L. Kuchariková L. Materials. 2022;15:8543–8554. doi: 10.3390/ma15238543. [DOI] [PMC free article] [PubMed] [Google Scholar]
- Eskalen H. Uruş S. Kavgacı M. Kalmış H. V. Tahta B. Biomass Convers. Biorefin. 2024;14:1201–1214. doi: 10.1007/s13399-023-04048-5. [DOI] [Google Scholar]
- Bao X. Liu Z. Tian Z. Sun W. Wang H. Yuan X. J. Lumin. 2024;267:120408–120417. doi: 10.1016/j.jlumin.2023.120408. [DOI] [Google Scholar]
- Gallardo J. Durán A. de Damborenea J. J. Corros. Sci. 2004;46:795–806. doi: 10.1016/S0010-938X(03)00185-9. [DOI] [Google Scholar]
- Velázquez-González C. E. Martínez-Baltodano F. J. López-Cuevas J. Vargas-Gutiérrez G. Metals. 2024;14:77–94. doi: 10.3390/met14010077. [DOI] [Google Scholar]
- Mumtaz K. Takahashi S. Echigoya J. Zhang L. Kamada Y. Sato M. J. Mater. Sci. Lett. 2003;22:423–427. doi: 10.1023/A:1022999309138. [DOI] [Google Scholar]
- Chen A. Y. Zhang J. B. Song H. W. Lu J. Surf. Coat. Technol. 2007;201:7462–7466. doi: 10.1016/j.surfcoat.2007.02.018. [DOI] [Google Scholar]
- He S. Jiang D. Sun Z. Int. J. Electrochem. Sci. 2018;13:4700–4719. doi: 10.20964/2018.05.11. [DOI] [Google Scholar]
- Liu X. Guo Y. Wang Y. Pang L. Fu B. J. Mater. Sci. 2024;59:21974–21986. doi: 10.1007/s10853-024-10476-z. [DOI] [Google Scholar]
- Shahaly O. M. E. Abdel-Rahman A. A. H. Abd El-Sattar N. E. A. El-sayed H. A. Abdelshafi N. S. J. Ind. Eng. Chem. 2026;160:246–280. doi: 10.1016/j.jiec.2026.01.038. [DOI] [Google Scholar]
- Ma G. Xu J. Han L. Xu Y. Corros. Sci. 2022;204:110387–110397. doi: 10.1016/j.corsci.2022.110387. [DOI] [Google Scholar]
- Elsamman A. Abdelshafi N. S. El-kazak A. M. El-mahdy K. M. Khaled K. F. Moroccan J. Chem. 2026;14:914–958. [Google Scholar]
- Abdelshafi N. S. Sadik M. A. Shoeib M. A. Halim S. A. Arabian J. Chem. 2022;15:103459–103485. doi: 10.1016/j.arabjc.2021.103459. [DOI] [Google Scholar]
- Elsamman A. Khaled K. F. Halim S. A. Abdelshafi N. S. J. Mol. Struct. 2023;1293:136230–136251. doi: 10.1016/j.molstruc.2023.136230. [DOI] [Google Scholar]
- Emrayed H. F. Amraga E. A. Ibrahim D. M. Fouda A. E.-A. S. Int. J. Electrochem. Sci. 2025;20:100912–100929. doi: 10.1016/j.ijoes.2024.100912. [DOI] [Google Scholar]
- Amrani Z. Barrahi A. Farag A. A. Thakur A. El Faydy M. Kaichouh G. Safi Z. Wazzan N. Warad I. Zarrouk A. Colloids Surf., A. 2025;709:136079–136096. doi: 10.1016/j.colsurfa.2024.136079. [DOI] [Google Scholar]
- Toghan A. Abdelshafi N. S. Zaki M. E. A. Abdel-Raouf M. E.-S. Farag A. A. J. Mol. Struct. 2026;1352:144556–144573. doi: 10.1016/j.molstruc.2025.144556. [DOI] [Google Scholar]
- Farag A. A. Tawfik S. M. Abd-Elaal A. A. Abdelshafi N. S. J. Ind. Eng. Chem. 2024;138:237–255. doi: 10.1016/j.jiec.2024.03.056. [DOI] [Google Scholar]
- Zhang Q. H. Xu N. Jiang Z. N. Liu H. F. Zhang G. A. J. Colloid Interface Sci. 2023;640:1052–1067. doi: 10.1016/j.jcis.2023.02.141. [DOI] [PubMed] [Google Scholar]
- Vaghefinazari B. Lamaka S. V. Blawert C. Serdechnova M. Scharnagl N. Karlova P. Wieland D. C. F. Zheludkevich M. L. Corros. Sci. 2022;203:110344–110360. doi: 10.1016/j.corsci.2022.110344. [DOI] [Google Scholar]
- Xu Y. Liu M. Geothermics. 2017;70:339–350. doi: 10.1016/j.geothermics.2017.08.001. [DOI] [Google Scholar]
- Farag A. A. Al-Shomar S. M. Abdelshafi N. S. Int. J. Biol. Macromol. 2024;279:135408–135425. doi: 10.1016/j.ijbiomac.2024.135408. [DOI] [PubMed] [Google Scholar]
Associated Data
This section collects any data citations, data availability statements, or supplementary materials included in this article.
Supplementary Materials
Data Availability Statement
The datasets used and/or analyzed during the current study are available from the corresponding author on reasonable request.
Supplementary information (SI): the raw electrochemical data and curves obtained from the electrochemical techniques used in this study. See DOI: https://doi.org/10.1039/d6ra08713b.